Lithium-rich manganese-based precursor, preparation method and application
Through the coordinated combination of two precipitants and two complexing agents, lithium-rich manganese-based precursors were prepared, which solved the problems of low firing rate and poor circulation performance of large-particle ternary nickel-cobalt manganese materials in lithium batteries, and achieved the A cathode material with high energy density and good cycle performance.
Patent Information
- Application Number
- CN202410989292.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The sintering rate of large-particle ternary nickel-cobalt manganese materials in the existing lithium battery industry is low, the electrochemical performance is not ideal, and the circulation performance of lithium-rich manganese-based precursors is poor, making it difficult to meet the needs of high energy density and good circulation performance. .
The coordinated combination method of two precipitant agents and two complexing agents is adopted to perform co-precipitation reaction by gradually adjusting the flow rate of the precipitant and complexing agent, and a lithium-rich manganese-based precursor is prepared to increase its specific surface area and tap density. This improves the energy density and cycling performance of the cathode material.
The specific surface area and tap density of the precursor material are significantly improved, the energy density and cyclic performance of the cathode material are improved, and efficient electrochemical performance is ensured.
Smart Images

Figure CN118908305A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries and relates to a lithium-rich manganese-based precursor, a preparation method and an application thereof. Background Art
[0002] At present, the ternary materials produced in the lithium battery industry include large-particle ternary nickel-cobalt-manganese materials. The conventional production method includes: dissolving nickel sulfate, cobalt sulfate, and manganese sulfate to form a mixed solution, and adding it to a reactor stirred at a certain stirring speed in parallel with ammonia water and sodium hydroxide. Among them, ammonia water plays a complexing role, so that the three ions of nickel, cobalt, and manganese maintain a similar concentration; sodium hydroxide provides hydroxide. After precipitation to obtain the co-precipitation nucleus of nickel, cobalt, and manganese hydroxide, the complexed nickel, cobalt, and manganese ions are continuously ionized to ensure that the concentration of nickel, cobalt, and manganese ions in the solution is stable during the growth of nickel, cobalt, and manganese hydroxide crystals.
[0003] However, this method has the problem of element segregation, and for large-particle ternary nickel-cobalt-manganese precursors, when the lithium source is sintered with the lithium source, it is difficult for the lithium source to enter the large-radius single crystal precursor material, resulting in a low sintering rate and unsatisfactory electrochemical performance. Moreover, the positive electrode material obtained from the lithium-rich manganese-based precursor provided by the prior art has a high capacity but poor cycle performance. Therefore, it is necessary to provide a small-particle lithium-rich manganese-based precursor with good cycle performance, a preparation method and application. Summary of the invention
[0004] The object of the present invention is to provide a lithium-rich manganese-based precursor, a preparation method and an application thereof. The preparation method can improve the specific surface area and tap density of the lithium-rich manganese-based precursor, and improve the energy density and cycle performance of the corresponding positive electrode material.
[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a lithium-rich manganese-based precursor, the preparation method comprising the following steps:
[0007] (1) a metal salt solution, a first precipitant solution, and a first complexing agent solution are simultaneously introduced into a base solution to perform a first coprecipitation reaction;
[0008] (2) then gradually reducing the flow rate of the first precipitant solution and the first complexing agent solution, and starting to flow the second precipitant solution and the second complexing agent solution in parallel to perform a second coprecipitation reaction;
[0009] (3) then stopping adding the first precipitant solution and the first complexing agent solution, and performing a third coprecipitation reaction to a target particle size to obtain the lithium-rich manganese-based precursor;
[0010] The first precipitant solution is a 9-12 mol / L sodium hydroxide solution, for example, 9 mol / L, 10 mol / L, 11 mol / L or 12 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0011] The second precipitant solution is a sodium carbonate solution of 180-220 g / L, for example, 180 g / L, 190 g / L, 200 g / L, 210 g / L or 220 g / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0012] The first complexing agent solution is an 8-10 mol / L ammonia solution, for example, 8 mol / L, 9 mol / L or 10 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0013] The concentration of the second complexing agent solution is 25-35 g / L, for example, it can be 25 g / L, 28 g / L, 30 g / L, 32 g / L or 35 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, wherein the second complexing agent includes citric acid and / or sodium citrate.
[0014] The preparation method provided by the present invention improves the specific surface area and tap density of the obtained precursor material and improves the energy density and cycle performance of the corresponding positive electrode material through the coordinated cooperation of two precipitants and two complexing agents; when any precipitant or any complexing agent is missing, the improvement of the precursor performance of the present invention cannot be achieved.
[0015] The gradual reduction means that the feed flow rate of the first precipitant solution is gradually reduced at a rate of 5-15% per hour, and the feed flow rate of the second precipitant solution is gradually increased.
[0016] The preparation method provided by the present invention is particularly suitable for lithium-rich manganese-based precursors.
[0017] Preferably, the metal salt in the metal salt solution includes nickel salt and cobalt salt and / or manganese salt, wherein the total molar concentration of the metal salt is 1.6-2.4 mol / L, for example, it can be 1.6 mol / L, 1.8 mol / L, 2 mol / L, 2.2 mol / L or 2.4 mol / L, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0018] Preferably, in the metal salt solution, the molar ratio of Ni, Co and Mn satisfies Ni:Co:Mn=x:y:c, and x+y+c=1, 0.2 <x<0.5,0.01≤y<0.1,0.5<c<0.8。
[0019] Preferably, the nickel salt comprises any one of nickel sulfate, nickel nitrate or nickel chloride or a combination of at least two thereof, typical but non-limiting combinations comprising a combination of nickel sulfate and nickel nitrate, a combination of nickel nitrate and nickel chloride, a combination of nickel sulfate and nickel chloride, or a combination of nickel sulfate, nickel nitrate and nickel chloride.
[0020] Preferably, the cobalt salt comprises any one of cobalt sulfate, cobalt nitrate or cobalt chloride or a combination of at least two thereof, typical but non-limiting combinations comprising a combination of cobalt sulfate and cobalt nitrate, a combination of cobalt nitrate and cobalt chloride, a combination of cobalt sulfate and cobalt chloride, or a combination of cobalt sulfate, cobalt nitrate and cobalt chloride.
[0021] Preferably, the manganese salt comprises any one or a combination of at least two of manganese sulfate, manganese nitrate or manganese chloride. Typical but non-limiting combinations include a combination of manganese sulfate and manganese nitrate, a combination of manganese nitrate and manganese chloride, a combination of manganese sulfate and manganese chloride, or a combination of manganese sulfate, manganese nitrate and manganese chloride.
[0022] Preferably, the base liquid is prepared from ammonia water, sodium hydroxide and water;
[0023] Preferably, the pH value of the base solution is 9-12, for example, 9, 10, 11 or 12, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the concentration of aqueous ammonia in the base liquid is 2-10 g / L, for example, 2 g / L, 4 g / L, 5 g / L, 6 g / L, 8 g / L or 10 g / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the temperature of the base liquid is 40-60°C, for example, 40°C, 45°C, 50°C, 55°C or 60°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] The pH value of the first coprecipitation reaction in step (1) is 10.3-11.5, for example, it can be 10.3, 10.5, 10.8, 11 or 11.5, but is not limited to the listed values, and the remaining values within the numerical range not listed are also applicable.
[0027] Preferably, during the first coprecipitation reaction in step (1), the concentration of aqueous ammonia in the system is 3-8 g / L, for example, 3 g / L, 4 g / L, 5 g / L, 6 g / L or 8 g / L, but is not limited to the listed values, and the remaining values not listed within the numerical range are also applicable.
[0028] Preferably, the first coprecipitation reaction in step (1) is carried out under stirring conditions of 200-500 rpm, for example, 200 rpm, 300 rpm, 400 rpm or 500 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] Preferably, the time of the first coprecipitation reaction in step (1) is 5-8 h, for example, 5 h, 6 h, 7 h or 8 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the pH value of the second coprecipitation reaction in step (2) is 9.5-11, for example, it can be 9.5, 9.8, 10, 10.5 or 11, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, during the second coprecipitation reaction in step (2), the concentration of aqueous ammonia in the system is 2-5 g / L, for example, 2 g / L, 3 g / L, 4 g / L or 5 g / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0032] Preferably, during the second coprecipitation reaction in step (2), the concentration of the second complexing agent in the system is 3-8 g / L, for example, 3 g / L, 4 g / L, 5 g / L, 6 g / L or 8 g / L, but is not limited to the listed values, and the remaining values within the numerical range not listed are also applicable.
[0033] Preferably, the second coprecipitation reaction in step (2) is carried out under stirring conditions of 200-500 rpm, for example, 200 rpm, 300 rpm, 400 rpm or 500 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] Preferably, the time of the second coprecipitation reaction in step (2) is 7-9 h, for example, 7 h, 7.5 h, 8 h, 8.5 h or 9 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] Preferably, the pH value of the third coprecipitation reaction in step (3) is 9-9.8, for example, it can be 9, 9.3, 9.5, 9.6 or 9.8, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] Preferably, during the third coprecipitation reaction in step (3), the concentration of the second complexing agent in the system is 0.5-3.5 g / L, for example, 0.5 g / L, 1.5 g / L, 2.5 g / L, 3 g / L or 3.5 g / L, but is not limited to the listed values, and the remaining values within the numerical range not listed are also applicable.
[0037] Preferably, the third coprecipitation reaction in step (3) is carried out under stirring conditions of 200-500 rpm, for example, 200 rpm, 300 rpm, 400 rpm or 500 rpm, but is not limited to the listed values, and the remaining values not listed within the numerical range are also applicable.
[0038] Preferably, the time of the third coprecipitation reaction in step (3) is 7-9 h, for example, 7 h, 7.5 h, 8 h, 8.5 h or 9 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0039] Preferably, the target particle size in step (3) refers to a particle size D50 of 8-12 μm, for example, 8 μm, 9 μm, 10 μm, 11 μm or 12 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] The preparation method provided by the present invention also includes conventional solid-liquid separation, washing, drying and removal of magnetic foreign matter.
[0041] Preferably, the preparation method is carried out in a mixed atmosphere of nitrogen and oxygen.
[0042] As a preferred technical solution of the preparation method provided in the first aspect of the present invention, the preparation method comprises the following steps:
[0043] (1) a metal salt solution, a first precipitant solution, and a first complexing agent solution are simultaneously introduced into a base solution to perform a first coprecipitation reaction;
[0044] The base liquid is prepared from ammonia water, sodium hydroxide and water, with a pH value of 9-12, a concentration of ammonia water of 2-10 g / L, and a temperature of 40-60° C.;
[0045] The pH value of the first coprecipitation reaction is 10.3-11.5, and the concentration of ammonia water in the system is 3-8 g / L; the first coprecipitation reaction is carried out under stirring conditions of 200-500 rpm for 5-8 hours;
[0046] (2) then gradually reducing the flow rate of the first precipitant solution and the first complexing agent solution, and starting to flow the second precipitant solution and the second complexing agent solution in parallel to perform a second coprecipitation reaction;
[0047] The pH value of the second coprecipitation reaction is 9.5-11, the concentration of ammonia water in the system is 2-5 g / L, and the concentration of the second complexing agent in the system is 3-8 g / L; the second coprecipitation reaction is carried out under stirring conditions of 200-500 rpm for 7-9 hours;
[0048] (3) then stopping adding the first precipitant solution and the first complexing agent solution, and performing a third coprecipitation reaction until the target particle size D50 is 8-12 μm, thereby obtaining the lithium-rich manganese-based precursor;
[0049] The pH value of the third coprecipitation reaction is 9-9.8, and the concentration of the second complexing agent in the system is 0.5-3.5 g / L; the third coprecipitation reaction is carried out under stirring conditions of 200-500 rpm for 7-9 hours;
[0050] The first precipitant solution is a 9-12 mol / L sodium hydroxide solution;
[0051] The second precipitant solution is a 180-220 g / L sodium carbonate solution;
[0052] The first complexing agent solution is an 8-10 mol / L ammonia solution;
[0053] The concentration of the second complexing agent solution is 25-35 g / L, wherein the second complexing agent includes citric acid and / or sodium citrate.
[0054] In a second aspect, the present invention provides a lithium-rich manganese-based precursor, and the lithium-rich manganese-based precursor is obtained by the preparation method described in the first aspect.
[0055] In a third aspect, the present invention provides a positive electrode material, wherein the lithium-rich manganese-based precursor is obtained by mixing and sintering a lithium source with the lithium-rich manganese-based precursor described in the second aspect.
[0056] Preferably, the lithium source comprises lithium hydroxide and / or lithium carbonate.
[0057] The amount of lithium source added is slightly higher than the theoretical amount to compensate for the loss on ignition caused by sintering.
[0058] Preferably, the sintering comprises: mixing the heat-treated lithium-rich manganese-based precursor with a lithium source, and then heating the mixture to 840-860° C. at a rate of 4-6° C. / min and sintering the mixture for 8-10 hours.
[0059] The heating rate of the sintering is 4-6°C / min, for example, 4°C / min, 5°C / min or 6°C / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0060] The sintering temperature is 840-860° C., for example, 840° C., 850° C. or 860° C., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0061] The sintering time is 8-10 hours, for example, 8 hours, 9 hours or 10 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0062] Preferably, the heat treatment is carried out in an air atmosphere at a temperature of 340-360° C. for a time of 2.5-3.5 h.
[0063] The temperature of the heat treatment is 340-360° C., for example, 340° C., 350° C. or 360° C., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0064] The heat treatment time is 2.5-3.5 h, for example, 2.5 h, 2.8 h, 3 h, 3.2 h or 3.5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0065] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the positive electrode material described in the third aspect.
[0066] Compared with the prior art, the present invention has the following beneficial effects:
[0067] The preparation method provided by the present invention improves the specific surface area and tap density of the obtained precursor material and improves the energy density and cycle performance of the corresponding positive electrode material through the coordinated cooperation of two precipitants and two complexing agents; when any precipitant or any complexing agent is missing, the improvement of the precursor performance of the present invention cannot be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] Figure 1 This is a SEM image of the lithium-rich manganese-based precursor obtained in Example 1. DETAILED DESCRIPTION
[0069] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0070] Example 1
[0071] This embodiment provides a method for preparing a lithium-rich manganese-based precursor, the preparation method comprising the following steps:
[0072] (1) In a mixed atmosphere of nitrogen and oxygen, a metal salt solution, a first precipitant solution, and a first complexing agent solution are simultaneously introduced into a base liquid to perform a first coprecipitation reaction;
[0073] The metal salt in the metal salt solution includes nickel sulfate, cobalt sulfate and manganese sulfate, the total molar concentration of nickel, cobalt and manganese is 2 mol / L, and the molar ratio of nickel, cobalt and manganese is 39:1:60;
[0074] The base liquid is prepared from ammonia water, sodium hydroxide and water, with a pH value of 11.5, an ammonia concentration of 6 g / L and a temperature of 50°C;
[0075] The pH value of the first coprecipitation reaction was 11, and the concentration of aqueous ammonia in the system was 5 g / L; the first coprecipitation reaction was carried out under stirring conditions of 380 rpm for 6 hours;
[0076] (2) gradually reducing the first precipitant solution, adjusting the flow rate of the first complexing agent solution, and starting to flow the second precipitant solution and the second complexing agent solution in parallel to perform a second coprecipitation reaction;
[0077] The gradually decreasing means gradually decreasing the feed flow rate of the first precipitant solution at a rate of 8.5% per hour, and gradually increasing the feed flow rate of the second precipitant solution;
[0078] The pH value of the second coprecipitation reaction is 10, the concentration of ammonia water in the system is 3.5 g / L, and the concentration of the second complexing agent in the system is 5.5 g / L; the second coprecipitation reaction is carried out under stirring conditions of 380 rpm for 8 hours;
[0079] (3) then stopping adding the first precipitant solution and the first complexing agent solution, and performing a third coprecipitation reaction until the target particle size D50 is 10 μm, thereby obtaining the lithium-rich manganese-based precursor;
[0080] The pH value of the third coprecipitation reaction was 9.5, and the concentration of the second complexing agent in the system was 2 g / L; the third coprecipitation reaction was carried out under stirring at 380 rpm for 8 hours;
[0081] The first precipitant solution is a 10 mol / L sodium hydroxide solution;
[0082] The second precipitant solution is a 200 g / L sodium carbonate solution;
[0083] The first complexing agent solution is a 9 mol / L ammonia solution;
[0084] The concentration of the second complexing agent solution is 30 g / L, wherein the second complexing agent is citric acid.
[0085] The SEM image of the lithium-rich manganese-based precursor obtained in this example is as follows Figure 1 shown.
[0086] Example 2
[0087] This embodiment provides a method for preparing a lithium-rich manganese-based precursor, the preparation method comprising the following steps:
[0088] (1) In a mixed atmosphere of nitrogen and oxygen, a metal salt solution, a first precipitant solution, and a first complexing agent solution are simultaneously introduced into a base liquid to perform a first coprecipitation reaction;
[0089] The metal salt in the metal salt solution includes nickel sulfate and manganese sulfate, the total molar concentration of nickel and manganese is 2.4 mol / L, and the molar ratio of nickel to manganese is 40:60;
[0090] The base liquid is prepared from ammonia water, sodium hydroxide and water, with a pH value of 12, an ammonia concentration of 10 g / L and a temperature of 60°C;
[0091] The pH value of the first coprecipitation reaction was 11.5, and the concentration of aqueous ammonia in the system was 8 g / L; the first coprecipitation reaction was carried out under stirring conditions of 500 rpm for 5 hours;
[0092] (2) gradually reducing the first precipitant solution, adjusting the flow rate of the first complexing agent solution, and starting to flow the second precipitant solution and the second complexing agent solution in parallel to perform a second coprecipitation reaction;
[0093] The gradually decreasing means gradually decreasing the feed flow rate of the first precipitant solution at a rate of 5% per hour, and gradually increasing the feed flow rate of the second precipitant solution;
[0094] The pH value of the second coprecipitation reaction is 11, the concentration of ammonia water in the system is 5 g / L, and the concentration of the second complexing agent in the system is 8 g / L; the second coprecipitation reaction is carried out under stirring conditions of 500 rpm for 7 hours;
[0095] (3) then stopping adding the first precipitant solution and the first complexing agent solution, and performing a third coprecipitation reaction until the target particle size D50 is 12 μm, thereby obtaining the lithium-rich manganese-based precursor;
[0096] The pH value of the third coprecipitation reaction was 9.8, and the concentration of the second complexing agent in the system was 3.5 g / L; the third coprecipitation reaction was carried out under stirring at 500 rpm for 7 hours;
[0097] The first precipitant solution is a 12 mol / L sodium hydroxide solution;
[0098] The second precipitant solution is a 220 g / L sodium carbonate solution;
[0099] The first complexing agent solution is a 10 mol / L ammonia solution;
[0100] The concentration of the second complexing agent solution is 35 g / L, wherein the second complexing agent is citric acid.
[0101] Example 3
[0102] This embodiment provides a method for preparing a lithium-rich manganese-based precursor, the preparation method comprising the following steps:
[0103] (1) In a mixed atmosphere of nitrogen and oxygen, a metal salt solution, a first precipitant solution, and a first complexing agent solution are simultaneously introduced into a base liquid to perform a first coprecipitation reaction;
[0104] The metal salt in the metal salt solution includes nickel sulfate, cobalt sulfate and manganese sulfate, the total molar concentration of nickel, cobalt and manganese is 1.6 mol / L, and the molar ratio of nickel, cobalt and manganese is 35:2:63;
[0105] The base liquid is prepared from ammonia water, sodium hydroxide and water, with a pH value of 9, an ammonia concentration of 2 g / L and a temperature of 40°C;
[0106] The pH value of the first coprecipitation reaction was 10.3, and the concentration of aqueous ammonia in the system was 3 g / L; the first coprecipitation reaction was carried out under stirring conditions of 200 rpm for 8 hours;
[0107] (2) gradually reducing the first precipitant solution, adjusting the flow rate of the first complexing agent solution, and starting to flow the second precipitant solution and the second complexing agent solution in parallel to perform a second coprecipitation reaction;
[0108] The gradually decreasing means gradually decreasing the feed flow rate of the first precipitant solution at a rate of 15% per hour, and gradually increasing the feed flow rate of the second precipitant solution;
[0109] The pH value of the second coprecipitation reaction was 9.5, the concentration of ammonia water in the system was 2 g / L, and the concentration of the second complexing agent in the system was 3 g / L; the second coprecipitation reaction was carried out under stirring at 200 rpm for 9 hours;
[0110] (3) then stopping adding the first precipitant solution and the first complexing agent solution, and performing a third coprecipitation reaction until the target particle size D50 is 8 μm, thereby obtaining the lithium-rich manganese-based precursor;
[0111] The pH value of the third coprecipitation reaction is 9, and the concentration of the second complexing agent in the system is 0.5 g / L; the third coprecipitation reaction is carried out under stirring conditions of 200 rpm for 7 hours;
[0112] The first precipitant solution is a 9 mol / L sodium hydroxide solution;
[0113] The second precipitant solution is a 180 g / L sodium carbonate solution;
[0114] The first complexing agent solution is an 8 mol / L ammonia solution;
[0115] The concentration of the second complexing agent solution is 25 g / L, wherein the second complexing agent is sodium citrate.
[0116] Comparative Example 1
[0117] This comparative example provides a method for preparing a lithium-rich manganese-based precursor, the preparation method comprising the following steps:
[0118] (1) In a mixed atmosphere of nitrogen and oxygen, a metal salt solution, a second precipitant solution, and a first complexing agent solution are simultaneously introduced into the base liquid to perform a first coprecipitation reaction;
[0119] The metal salt in the metal salt solution includes nickel sulfate, cobalt sulfate and manganese sulfate, the total molar concentration of nickel, cobalt and manganese is 2 mol / L, and the molar ratio of nickel, cobalt and manganese is 39:1:60;
[0120] The base liquid is prepared from ammonia water, sodium carbonate and water, with a pH value of 10, an ammonia concentration of 6 g / L and a temperature of 50°C;
[0121] The pH value of the first coprecipitation reaction was 11, and the concentration of aqueous ammonia in the system was 5 g / L; the first coprecipitation reaction was carried out under stirring conditions of 380 rpm for 6 hours;
[0122] (2) then reducing the flow rate of the first complexing agent solution and beginning to introduce the second complexing agent solution to perform a second coprecipitation reaction;
[0123] The pH value of the second coprecipitation reaction is 10, the concentration of ammonia water in the system is 3.5 g / L, and the concentration of the second complexing agent in the system is 5.5 g / L; the second coprecipitation reaction is carried out under stirring conditions of 380 rpm for 8 hours;
[0124] (3) then stopping the addition of the first complexing agent solution, and performing a third coprecipitation reaction until the target particle size D50 is 10 μm, to obtain the lithium-rich manganese-based precursor;
[0125] The pH value of the third coprecipitation reaction was 9.5, and the concentration of the second complexing agent in the system was 2 g / L; the third coprecipitation reaction was carried out under stirring at 380 rpm for 8 hours;
[0126] The second precipitant solution is a 200 g / L sodium carbonate solution;
[0127] The first complexing agent solution is a 9 mol / L ammonia solution;
[0128] The concentration of the second complexing agent solution is 30 g / L, wherein the second complexing agent is citric acid.
[0129] Comparative Example 2
[0130] This comparative example provides a method for preparing a lithium-rich manganese-based precursor, the preparation method comprising the following steps:
[0131] (1) In a mixed atmosphere of nitrogen and oxygen, a metal salt solution, a first precipitant solution, and a first complexing agent solution are simultaneously introduced into a base liquid to perform a first coprecipitation reaction;
[0132] The metal salt in the metal salt solution includes nickel sulfate, cobalt sulfate and manganese sulfate, the total molar concentration of nickel, cobalt and manganese is 2 mol / L, and the molar ratio of nickel, cobalt and manganese is 39:1:60;
[0133] The base liquid is prepared from ammonia water, sodium hydroxide and water, with a pH value of 10, an ammonia concentration of 6 g / L and a temperature of 50°C;
[0134] The pH value of the first coprecipitation reaction was 11, and the concentration of aqueous ammonia in the system was 5 g / L; the first coprecipitation reaction was carried out under stirring conditions of 380 rpm for 6 hours;
[0135] (2) then reducing the flow rate of the first complexing agent solution and beginning to introduce the second complexing agent solution to perform a second coprecipitation reaction;
[0136] The pH value of the second coprecipitation reaction is 10, the concentration of ammonia water in the system is 3.5 g / L, and the concentration of the second complexing agent in the system is 5.5 g / L; the second coprecipitation reaction is carried out under stirring conditions of 380 rpm for 8 hours;
[0137] (3) then stopping the addition of the first complexing agent solution, and performing a third coprecipitation reaction until the target particle size D50 is 10 μm, to obtain the lithium-rich manganese-based precursor;
[0138] The pH value of the third coprecipitation reaction was 9.5, and the concentration of the second complexing agent in the system was 2 g / L; the third coprecipitation reaction was carried out under stirring at 380 rpm for 8 hours;
[0139] The first precipitant solution is a 10 mol / L sodium hydroxide solution;
[0140] The first complexing agent solution is a 9 mol / L ammonia solution;
[0141] The concentration of the second complexing agent solution is 30 g / L, wherein the second complexing agent is citric acid.
[0142] Comparative Example 3
[0143] This comparative example provides a method for preparing a lithium-rich manganese-based precursor, the preparation method comprising the following steps:
[0144] (1) In a mixed atmosphere of nitrogen and oxygen, a metal salt solution, a first precipitant solution, and a second complexing agent solution are simultaneously introduced into a base liquid to perform a first coprecipitation reaction;
[0145] The metal salt in the metal salt solution includes nickel sulfate, cobalt sulfate and manganese sulfate, the total molar concentration of nickel, cobalt and manganese is 2 mol / L, and the molar ratio of nickel, cobalt and manganese is 39:1:60;
[0146] The base liquid is prepared from citric acid, sodium hydroxide and water, with a pH value of 10, a concentration of citric acid of 6 g / L and a temperature of 50°C;
[0147] The pH value of the first coprecipitation reaction was 11, and the concentration of citric acid in the system was 5 g / L; the first coprecipitation reaction was carried out under stirring conditions of 380 rpm for 6 hours;
[0148] (2) then gradually reducing the flow rate of the first precipitant solution, and starting to flow the second precipitant solution in parallel to perform a second coprecipitation reaction;
[0149] The gradually decreasing means gradually decreasing the feed flow rate of the first precipitant solution at a rate of 8.5% per hour, and gradually increasing the feed flow rate of the second precipitant solution;
[0150] The pH value of the second coprecipitation reaction was 10, and the concentration of citric acid in the system was 5.5 g / L; the second coprecipitation reaction was carried out under stirring conditions of 380 rpm for 8 hours;
[0151] (3) then stopping the addition of the first precipitant solution, and performing a third coprecipitation reaction until the target particle size D50 is 10 μm, to obtain the lithium-rich manganese-based precursor;
[0152] The pH value of the third coprecipitation reaction was 9.5, and the concentration of citric acid in the system was 2 g / L; the third coprecipitation reaction was carried out under stirring conditions of 380 rpm for 8 hours;
[0153] The first precipitant solution is a 10 mol / L sodium hydroxide solution;
[0154] The second precipitant solution is a 200 g / L sodium carbonate solution;
[0155] The concentration of the second complexing agent solution is 30 g / L, wherein the second complexing agent is citric acid.
[0156] Comparative Example 4
[0157] This comparative example provides a method for preparing a lithium-rich manganese-based precursor, the preparation method comprising the following steps:
[0158] (1) In a mixed atmosphere of nitrogen and oxygen, a metal salt solution, a first precipitant solution, and a first complexing agent solution are simultaneously introduced into a base liquid to perform a first coprecipitation reaction;
[0159] The metal salt in the metal salt solution includes nickel sulfate, cobalt sulfate and manganese sulfate, the total molar concentration of nickel, cobalt and manganese is 2 mol / L, and the molar ratio of nickel, cobalt and manganese is 39:1:60;
[0160] The base liquid is prepared from ammonia water, sodium hydroxide and water, with a pH value of 10, an ammonia concentration of 6 g / L and a temperature of 50°C;
[0161] The pH value of the first coprecipitation reaction was 11, and the concentration of aqueous ammonia in the system was 5 g / L; the first coprecipitation reaction was carried out under stirring conditions of 380 rpm for 6 hours;
[0162] (2) then gradually reducing the flow rate of the first precipitant solution, and starting to flow the second precipitant solution in parallel to perform a second coprecipitation reaction;
[0163] The gradually decreasing means gradually decreasing the feed flow rate of the first precipitant solution at a rate of 8.5% per hour, and gradually increasing the feed flow rate of the second precipitant solution;
[0164] The pH value of the second coprecipitation reaction was 10, and the concentration of aqueous ammonia in the system was 3.5 g / L; the second coprecipitation reaction was carried out under stirring conditions of 380 rpm for 8 hours;
[0165] (3) then stopping the addition of the first precipitant solution, and performing a third coprecipitation reaction until the target particle size D50 is 10 μm, to obtain the lithium-rich manganese-based precursor;
[0166] The pH value of the third coprecipitation reaction was 9.5, and the concentration of aqueous ammonia in the system was 2 g / L; the third coprecipitation reaction was carried out under stirring conditions of 380 rpm for 8 hours;
[0167] The first precipitant solution is a 10 mol / L sodium hydroxide solution;
[0168] The second precipitant solution is a 200 g / L sodium carbonate solution;
[0169] The first complexing agent solution is a 9 mol / L ammonia solution.
[0170] Performance Characterization
[0171] The specific surface area BET and tap density of the lithium-rich manganese-based precursors obtained in the above examples and comparative examples were measured; the results are shown in Table 1.
[0172] Table 1
[0173] <![CDATA[Specific surface area BET (m 2 / g)]]> <![CDATA[Tap density (g / cm 3 )]]> Example 1 71.4 1.93 Example 2 55.7 2.21 Example 3 65.3 2.08 Comparative Example 1 75.4 1.85 Comparative Example 2 6.5 2.0 Comparative Example 3 78.8 1.63 Comparative Example 4 22.5 1.73
[0174] The lithium-rich manganese-based precursors obtained in the above embodiments and comparative examples are prepared into positive electrode materials and assembled into button batteries: the lithium-rich manganese-based precursors are heat treated in an air atmosphere at 350°C for 3 hours, and then the lithium carbonate and the lithium-rich manganese-based precursors are evenly mixed, and then the temperature is raised to 850°C at a rate of 5°C / min and sintered for 9 hours to obtain the positive electrode material.
[0175] The positive electrode material, acetylene black and polyvinylidene fluoride were dropped into N-methyl-2-pyrrolidone in a mass ratio of 8:1:1 to prepare a solution, which was evenly applied on an aluminum foil, dried and punched into a pole piece; the pole piece, sodium sheet, glass fiber diaphragm, electrolyte (NaClO4) gasket, shrapnel and battery shell were assembled into a button battery in an Ar gas glove box, and its first discharge specific capacity and cycle capacity retention rate were measured. The results are shown in Table 2.
[0176] Among them, the test method for the first discharge specific capacity is at a temperature of 25℃±1℃, a voltage range of 2.0V-4.6V for the charge and discharge cycle, and a current of 0.1C;
[0177] The test method for 100-cycle cycle capacity retention rate is: the ratio of 1C discharge capacity after 100 cycles to the 1C discharge capacity after the first cycle.
[0178] Table 2
[0179] First discharge specific capacity (mAh / g) 100-cycle capacity retention rate (%) Example 1 280 88.4 Example 2 273 83.5 Example 3 272 86.7 Comparative Example 1 281 63.5 Comparative Example 2 253 92.5 Comparative Example 3 264 90.5 Comparative Example 4 256 89.7
[0180] In summary, the preparation method provided by the present invention improves the specific surface area and tap density of the obtained precursor material and improves the energy density and cycle performance of the corresponding positive electrode material through the synergistic combination of two precipitants and two complexing agents; when any precipitant or any complexing agent is missing, the improvement of the precursor performance of the present invention cannot be achieved.
[0181] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a lithium-rich manganese-based precursor, characterized in that: The preparation method comprises the following steps: (1) a metal salt solution, a first precipitant solution, and a first complexing agent solution are simultaneously introduced into a base solution to perform a first coprecipitation reaction; (2) then gradually reducing the flow rate of the first precipitant solution and the first complexing agent solution, and starting to flow the second precipitant solution and the second complexing agent solution in parallel to perform a second coprecipitation reaction; (3) then stopping adding the first precipitant solution and the first complexing agent solution, and performing a third coprecipitation reaction to a target particle size to obtain the lithium-rich manganese-based precursor; The first precipitant solution is a 9-12 mol / L sodium hydroxide solution; The second precipitant solution is a 180-220 g / L sodium carbonate solution; The first complexing agent solution is an 8-10 mol / L ammonia solution; The concentration of the second complexing agent solution is 25-35 g / L, wherein the second complexing agent includes citric acid and / or sodium citrate.
2. The preparation method according to claim 1, characterized in that: The base liquid is prepared from ammonia water, sodium hydroxide and water; Preferably, the pH value of the base solution is 9-12; Preferably, the concentration of ammonia water in the base solution is 2-10 g / L; Preferably, the temperature of the base liquid is 40-60°C.
3. The preparation method according to claim 1 or 2, characterized in that: The pH value of the first coprecipitation reaction in step (1) is 10.3-11.5; Preferably, during the first coprecipitation reaction in step (1), the concentration of aqueous ammonia in the system is 3-8 g / L; Preferably, the first coprecipitation reaction in step (1) is carried out under stirring conditions of 200-500 rpm; Preferably, the first coprecipitation reaction time in step (1) is 5-8 hours.
4. The preparation method according to any one of claims 1 to 3, characterized in that Step (2) the pH value of the second coprecipitation reaction is 9.5-11; Preferably, during the second coprecipitation reaction in step (2), the concentration of aqueous ammonia in the system is 2-5 g / L; Preferably, during the second coprecipitation reaction in step (2), the concentration of the second complexing agent in the system is 3-8 g / L; Preferably, the second coprecipitation reaction in step (2) is carried out under stirring conditions of 200-500 rpm; Preferably, the time of the second co-precipitation reaction in step (2) is 7-9 hours.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The pH value of the third coprecipitation reaction in step (3) is 9-9.8; Preferably, during the third coprecipitation reaction in step (3), the concentration of the second complexing agent in the system is 0.5-3.5 g / L; Preferably, the third coprecipitation reaction in step (3) is carried out under stirring conditions of 200-500 rpm; Preferably, the time of the third coprecipitation reaction in step (3) is 7-9 hours.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The target particle size in step (3) refers to a particle size D50 of 8-12 μm.
7. A lithium-rich manganese-based precursor, characterized in that: The lithium-rich manganese-based precursor is obtained by the preparation method according to any one of claims 1 to 6.
8. A positive electrode material, characterized in that The lithium-rich manganese-based precursor is obtained by mixing and sintering a lithium source with the lithium-rich manganese-based precursor according to claim 7.
9. The positive electrode material according to claim 8, characterized in that The sintering comprises: The heat-treated lithium-rich manganese-based precursor is mixed with a lithium source, and then heated to 840-860°C at a rate of 4-6°C / min and sintered for 8-10h; Preferably, the heat treatment is carried out in an air atmosphere at a temperature of 340-360° C. for a time of 2.5-3.5 h.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode material according to claim 8 or 9.
Citation Information
Patent Citations
Preparation method of double-layer composite low-cost lithium-rich manganese-based precursor
CN114455648A
Copper-containing multi-element sodium electric precursor, preparation method thereof, positive electrode material and sodium ion battery
CN116750805A
Iron-doped lithium-rich manganese-based precursor material as well as preparation method and application thereof
CN117534132A
Sodium ion precursor material with double concentration gradients and preparation method thereof
CN117566809A
Method for controlling oxidation degree of lithium-rich manganese-based precursor and lithium-rich manganese-based precursor
CN117776290A
Cited By
Iron-based single crystal positive electrode precursor as well as preparation method and application thereof
CN121134861A
An iron-based single-crystal positive electrode precursor, a preparation method therefor, and an application thereof
CN121134861B
High-nickel ternary precursor, lithium-rich positive electrode material, and preparation method
WO2026137621A1