Titanium-based nickel ruthenium bimetallic doped tin antimony electrode and preparation method and application thereof
Through the preparation of titanium-based nickel-ruthenium bimetal doped tin antimony electrode, the problems of low catalytic activity and short service life in the prior art are solved, efficient industrial wastewater treatment is achieved, and the stability and catalytic activity of the electrode are improved, and the stability and catalytic activity of the electrode are reduced. The cost.
Patent Information
- Application Number
- CN202411054840.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, anode materials with low catalytic activity and short service life are difficult to efficiently treat organic pollutants in industrial wastewater, and the preparation process is complex and costly.
Develop a titanium-based nickel-ruthenium bimetal doped tin antimony electrode, which is prepared by pretreatment of substrate material, precursor coating, drying and fixing, and calcining. The catalyst includes nickel, ruthenium, tin, and antimony, with a molar ratio of 1:1 To 4:1, the load capacity is 1.2~3.0 mg/cm2, and the preparation is repeated 10~20 times to improve the electrode performance.
The catalytic activity, corrosion resistance and service life of the electrode are improved, the efficiency of organic degradation is enhanced, the charge transfer resistance and oxygen evolution potential of the electrode are reduced, and the COD removal rate of wastewater treatment is improved.
Smart Images

Figure CN118908356A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical technology and electrode material preparation technology, and more specifically to a titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode and a preparation method and application thereof. Background Art
[0002] With the development of industry, the discharge of large amounts of industrial wastewater has become a serious environmental problem. These industrial wastewaters usually contain a large amount of organic pollutants. For example, pharmaceutical wastewater often contains various heterocyclic organic pollutants, while coking wastewater often contains phenolic organic pollutants. The structures of these organic pollutants are relatively stable, and traditional wastewater treatment methods are difficult to achieve efficient removal. Electrocatalytic oxidation technology can generate OH in situ, has extremely strong oxidation ability, can effectively destroy the molecular structure of organic pollutants, and achieve thorough mineralization. In addition, electrochemical oxidation technology also has the advantages of no need for reagent addition, no secondary pollution, and small footprint, showing great potential in industrial wastewater treatment.
[0003] Anode materials are the core of electrocatalytic oxidation technology. Active anodes such as graphite, platinum, ruthenium, iridium and titanium have low oxygen evolution potentials and strong oxygen evolution side reactions, so they have low catalytic oxidation activity for organic pollutants; while inactive electrodes such as tin antimony titanium and lead dioxide have poor corrosion resistance, and the catalytic layer is easy to fall off after long-term use, resulting in generally low service life; boron-doped diamond electrodes have high catalytic activity and long service life, but the complex preparation process and high price limit their large-scale application.
[0004] Therefore, there is an urgent need to develop an anode material with high catalytic activity, long service life, simple preparation process and low cost. Summary of the invention
[0005] 1. Technical problem to be solved by the invention
[0006] The purpose of the present invention is to overcome the shortcomings of low catalytic activity and short service life in the prior art, and provide a titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode, a preparation method of the electrode is provided, and the electrode is applied to wastewater treatment.
[0007] 2. Technical solution
[0008] In order to achieve the above object, the technical solution provided by the present invention is:
[0009] The titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode of the present invention comprises:
[0010] A titanium-containing substrate material and a catalyst supported on the substrate material;
[0011] The catalyst includes nickel and ruthenium;
[0012] The molar ratio of nickel to ruthenium is 1-4:1-4.
[0013] The molar ratio of nickel to ruthenium can specifically be 1:1, 1:2, 1:3, 1:4, 2:3, 3:2, 4:1, 3:1, or 2:1.
[0014] Preferably, the molar ratio of nickel to ruthenium is 1:1.
[0015] It should be noted that when the molar ratio of nickel to ruthenium is greater than 4:1, at this ratio, the nickel content is significantly higher than ruthenium. As an excellent catalyst, the high ratio of nickel helps to enhance the catalytic activity of the electrode, especially in promoting the efficiency of oxidation reactions. However, a higher ratio of nickel may also cause problems with the mechanical stability of the electrode, because nickel is more susceptible to changes in physical form during electrode operation, such as granulation or shedding, which may affect the long-term stability and service life of the electrode. When the molar ratio of nickel to ruthenium is less than 1:4, although ruthenium can provide better conductivity and physical stability, it is less active than nickel in the catalytic degradation of organic matter. Therefore, when the proportion of nickel is too high, although the electrode may exhibit better structural stability, its catalytic efficiency may not be optimal. This is because too much ruthenium may lead to an increase in the oxygen evolution side reaction, thereby affecting the electrode's ability to degrade organic matter, resulting in a suboptimal COD removal rate.
[0016] Furthermore, the catalyst also includes tin and antimony, and the molar ratio of tin, antimony, nickel and ruthenium is 120-240:6-10:1-4:1-4.
[0017] Furthermore, the catalyst loading on the substrate material is 1.2 to 3.0 mg / cm 2 .
[0018] Furthermore, the catalyst supported on the base material forms a catalytic layer.
[0019] The present invention also provides a method for preparing the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode, comprising the following steps:
[0020] S1, substrate pretreatment: grinding and etching the substrate material to obtain a pretreated substrate material;
[0021] S2, precursor liquid coating: evenly apply the precursor liquid containing nickel and ruthenium to the pretreated substrate material;
[0022] S3, drying and fixing: drying the coated substrate material;
[0023] S4, calcining: calcining the dried base material;
[0024] Wherein, the steps S2 to S4 are repeated N times to obtain a titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode;
[0025] In the step S2, the molar ratio of nickel to ruthenium in the precursor solution is 1-4:1-4.
[0026] Further, in the step S1, the polishing includes polishing with sandpaper of different types to remove the oxide layer on the surface;
[0027] The grinding sequence is to first grind with sandpaper of small mesh number and then grind with sandpaper of large mesh number.
[0028] Furthermore, in the step S1, the etching process is to perform acid etching on the polished base material using acid.
[0029] Furthermore, the acid used in the acid etching treatment is one, two or more of oxalic acid, nitric acid, hydrochloric acid and sulfuric acid;
[0030] Preferably, the acidic solution is an oxalic acid solution;
[0031] More preferably, the mass fraction of the oxalic acid solution is 5-10%.
[0032] Furthermore, the acid etching temperature is 80-95° C., and the time is 30-60 min.
[0033] Furthermore, the precursor solution also contains tin and antimony, and the molar ratio of tin, antimony, nickel and ruthenium in the precursor solution is 120-240:6-10:1-4:1-4.
[0034] For example, the molar concentrations of tin, antimony, nickel, and ruthenium in the precursor solution may be 450 mM, 20 mM, 2.5-10 mM, and 2.5-10 mM.
[0035] Furthermore, a precursor solution containing tin, antimony, nickel and ruthenium is obtained by dissolving a tin-containing compound, an antimony-containing compound, a nickel-containing compound and a ruthenium-containing compound.
[0036] Further, the tin-containing compound in the precursor solution is one, two or more of tin-containing metal chlorides, metal nitrates and metal carbonates;
[0037] The antimony-containing compound is one, two or more of antimony-containing metal chlorides, metal nitrates and metal carbonates;
[0038] The nickel-containing compound is one, two or more of nickel-containing metal chlorides, metal nitrates and metal carbonates;
[0039] The ruthenium-containing compound is one, two or more of ruthenium-containing metal chlorides, metal nitrates and metal carbonates.
[0040] Furthermore, the solvent of the precursor solution is one, two or three of ethanol, isopropanol and n-butanol.
[0041] Furthermore, in step S3, the drying process is carried out at a temperature of 80 to 95° C. and for a time of 5 to 20 minutes.
[0042] Furthermore, in step S4, the calcination temperature is 400-700° C. and the calcination time is 5-240 min.
[0043] Further, the value of N is 10 to 20; in the first N-1 times of step S4, the calcination temperature is 400 to 700° C. and the time is 5 to 20 min;
[0044] In the Nth step S4, the calcination temperature is 400-700° C. and the calcination time is 1-4 hours.
[0045] The present invention also provides an application of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode or the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode prepared by the above preparation method in wastewater treatment.
[0046] For example, the wastewater is one, two or more of pharmaceutical wastewater, coking wastewater or printing and dyeing wastewater.
[0047] 3. Beneficial effects
[0048] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0049] (1) The titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode provided by the present invention comprises a titanium-containing base material and a catalyst layer loaded on the base material; the catalyst layer comprises nickel, ruthenium, tin and antimony, and the catalyst layer is doped with transition metal nickel and precious metal ruthenium, so that the electrode has a higher electrode electrochemical active area and oxygen evolution potential and a lower charge transfer resistance, increases the number of reaction sites, and improves the corrosion resistance and electrocatalytic activity of the electrode.
[0050] (2) In the preparation method of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode provided by the present invention, steps S2 to S4 are repeated N times, wherein the value of N is 10 to 20. When the number of brushing times is too many, the thickness of the catalyst layer on the electrode surface may be too large, and the catalyst layer may also peel off, affecting the stability and service life of the electrode.
[0051] (3) The present invention applies the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode to wastewater treatment. Compared with the traditional tin-antimony-titanium electrode, the COD removal efficiency and service life of industrial wastewater such as pharmaceutical, coking and printing and dyeing are improved;
[0052] Moreover, since the oxygen evolution potential of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode is reduced, the electrochemical active area is increased, and the charge transfer resistance is reduced, the electrode shows higher performance in the degradation of organic matter. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 The SEM images of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrodes prepared in Example 1 and Comparative Examples 1-3 of the present invention;
[0054] Figure 2 The linear voltammetric scanning (LSV) curves of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrodes prepared in Example 1 and Comparative Examples 1-3 of the present invention;
[0055] Figure 3 The electrochemically active area (ECSA) curve of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode prepared in Example 1 and Comparative Examples 1-3 of the present invention;
[0056] Figure 4 It is an electrochemical impedance spectroscopy (EIS) curve of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode prepared in Example 1 and Comparative Examples 1-3 of the present invention. DETAILED DESCRIPTION
[0057] The present disclosure may be more easily understood by reference to the following description in conjunction with examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or illustrated herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise indicated.
[0058] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.
[0059] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".
[0060] In the present disclosure, the singular forms of the articles "a," "an," and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.
[0061] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.
[0062] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.
[0063] In general, the use of the term "about" indicates an approximate value that can vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to a value in a range includes each value within that range.
[0064] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.
[0065] The calculation formula for the loading amount of the catalyst layer in the embodiment of the present invention is:
[0066]
[0067] In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be purchased commercially.
[0068] The present invention is further described below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. The essential characteristics and remarkable effects of the present invention can be reflected from the following examples, and the described embodiments are part of the embodiments of the present invention, rather than all the embodiments, and therefore, they do not limit the present invention in any way, and those skilled in the art make some non-essential improvements and adjustments based on the content of the present invention, which all belong to the protection scope of the present invention.
[0069] Example 1
[0070] A titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode is prepared, comprising the following steps:
[0071] S1. Substrate pretreatment: Use sandpapers of 600 mesh and 1000 mesh to grind a titanium-containing substrate material (titanium plate, in which the titanium content is greater than 99%) with a length × width × thickness of 25 mm × 50 mm × 1 mm.
[0072] Then, 10% by mass oxalic acid was used for heating and etching at 90° C. for 45 min to obtain a pretreated substrate material;
[0073] S2. Precursor coating: Add SnCl4·5H2O, SbCl3, RuCl2·3H2O, NiCl2·6H2O to isopropanol, and make the concentrations 450mM, 20mM, 5mM and 5mM respectively, fully dissolve by ultrasonication to obtain a catalyst layer precursor solution, and then evenly apply the precursor solution to the pretreated substrate material;
[0074] S3, drying and fixing: drying the coated substrate material at 90°C for 10 min to fix the precursor liquid into a film on the titanium substrate;
[0075] S4, calcining: calcining the dried base material;
[0076] Steps S2 to S4 were repeated 15 times, and the calcination temperature in step S4 for the first 14 times was 550° C. and the time was 10 min; the calcination in step S4 for the 15th time was 550° C. for 2 h to obtain a titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode, and the loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode was 2 mg / cm 2 , and recorded as SnO2-Sb-Ru-Ni.
[0077] Example 2
[0078] The difference between this embodiment and embodiment 1 is that the concentration of RuCl2·3H2O is 2.5 mM, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode is 2 mg / cm 2 .
[0079] Example 3
[0080] The only difference between this embodiment and embodiment 1 is that the concentration of RuCl2·3H2O is 7.5 mM, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode is 2 mg / cm 2 .
[0081] Example 4
[0082] The difference between this embodiment and embodiment 1 is that the concentration of NiCl2·6H2O is 2.5 mM, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode is 2 mg / cm 2 .
[0083] Example 5
[0084] The difference between this embodiment and embodiment 1 is that the concentration of NiCl2·6H2O is 7.5 mM, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode is 2 mg / cm 2 .
[0085] Example 6
[0086] The difference between this embodiment and embodiment 1 is that the number of steps S2 to S4 is repeated 10 times, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode finally prepared is 1.3 mg / cm 2 .
[0087] Example 7
[0088] The difference between this embodiment and embodiment 1 is that the number of steps S2 to S4 is repeated 20 times, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode finally prepared is 2.7 mg / cm 2 .
[0089] Example 8
[0090] The difference between this embodiment and embodiment 1 is that the calcination temperature is 400°C when the calcination is repeated 15 times, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode finally prepared is 2 mg / cm 2 .
[0091] Example 9
[0092] The difference between this embodiment and embodiment 1 is that the calcination temperature is 700°C when the calcination is repeated 15 times, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode finally prepared is 2 mg / cm 2 .
[0093] Comparative Example 1
[0094] The difference between this comparative example and Example 1 is that RuCl2·3H2O and NiCl2·6H2O are not added to the precursor solution, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based tin-antimony electrode finally prepared is 2 mg / cm 2 , and recorded as SnO2-Sb.
[0095] Comparative Example 2
[0096] The difference between this comparative example and Example 1 is that RuCl2·3H2O is not added to the precursor solution, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-doped tin-antimony electrode finally prepared is 2 mg / cm 2 , and recorded as SnO2-Sb-Ni.
[0097] Comparative Example 3
[0098] The difference between this comparative example and Example 1 is that NiCl2·6H2O is not added to the precursor solution, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based ruthenium-doped tin-antimony electrode finally prepared is 2 mg / cm 2 , and recorded as SnO2-Sb-Ru.
[0099] Comparative Example 4
[0100] The difference between this comparative example and Example 1 is that SnCl4·5H2O and SbCl3 are not added to the precursor solution, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped electrode finally prepared is 0.02 mg / cm 2 .
[0101] Comparative Example 5
[0102] The difference between this comparative example and Example 1 is that the concentration of NiCl2·6H2O added is 1 mM, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode finally prepared is 2 mg / cm 2 .
[0103] Comparative Example 6
[0104] The difference between this comparative example and Example 1 is that the concentration of NiCl2·6H2O added is 25 mM, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode is 2 mg / cm 2 .
[0105] Comparative Example 7
[0106] The difference between this comparative example and Example 1 is that the number of steps S2 to S4 is repeated 6 times, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode finally prepared is 0.8 mg / cm 2 .
[0107] Comparative Example 8
[0108] The difference between this comparative example and Example 1 is that the number of steps S2 to S4 is repeated 25 times, and the other implementation conditions remain unchanged. The loading amount of the catalyst layer of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode finally prepared is 3.3 mg / cm 2 .
[0109] Degradation process: The electrocatalytic activity and service life of the electrodes prepared in the above embodiments and comparative examples were tested using three kinds of industrial wastewater, namely pharmaceutical, coking and printing and dyeing. Among them, the pollutants in pharmaceutical wastewater are mainly various antibiotics, such as tetracycline, carbamazepine, etc., with a COD of 8200 mg / L; the pollutants in coking wastewater are mainly various phenols and polycyclic aromatic hydrocarbons, with a COD of 12000 mg / L; the pollutants in printing and dyeing wastewater are mainly various dyes, such as orange G, rhodamine B, etc., with a COD of 8000 mg / L. The prepared electrode was used as the anode and the titanium plate as the cathode to repeat multiple batches of electrochemical oxidation reaction experiments, each batch reacting for 4 hours until the electrode was inactivated, that is, the internal resistance suddenly increased or the electrode was corroded. The COD removal rate of the electrode is the average COD removal rate of each batch; the service life is the total use time before the electrode is inactivated, that is, the number of batches × 4h. The plate spacing is 1cm, the wastewater volume is 100mL, and the current density is 30mA / cm 2 .
[0110] Table 1 Degradation of wastewater by electrodes in Example 1 and Comparative Examples 1-8
[0111]
[0112]
[0113] Table 2 Degradation of wastewater by electrodes of different embodiments
[0114]
[0115] Combining the data of Examples 1-5 and Comparative Examples 5 and 6 in Table 1 and Table 2, it can be seen that when the nickel ruthenium concentration is low, the initial increase in the concentration of nickel and ruthenium can improve the catalytic activity of the electrode, because the presence of these two metals can improve the electronic structure of the electrode surface and increase the effective catalytic sites. This will lead to an increase in COD removal efficiency and electrode life. When the nickel ruthenium concentration is high, when the concentration continues to increase above a certain threshold, the excessively high metal concentration may cause shielding of the active sites on the electrode surface or agglomeration of the catalyst, reducing the effective reaction surface area, and may increase the internal stress of the electrode, thereby reducing the COD removal efficiency and shortening the service life of the electrode.
[0116] Combining the data of Examples 1, 6, 7 and Comparative Examples 7, 8 in Table 1 and Table 2, it can be seen that the increase in the number of brushing times can increase the catalyst loading on the electrode surface in the initial stage, thereby improving the catalytic activity and surface area of the electrode, leading to an increase in COD removal rate and electrode life. When the number of brushing times is too many, the thickness of the catalyst layer on the electrode surface may be too large, and the catalyst layer may also peel off, affecting the stability and service life of the electrode. Combining the data of Examples 1, 8 and 9 in Table 1, an appropriate calcination temperature helps the crystallization and fixation of the catalyst on the electrode surface, thereby improving the structural stability and catalytic efficiency of the electrode. If the calcination temperature is too high, the catalyst structure may be over-hardened or even destroyed, reducing the catalytic activity. At the same time, high temperature may cause thermal stress in the material, further affecting the physical stability and chemical stability of the electrode.
[0117] Moreover, in comparison between Example 2 and Example 3, only a high content of nickel is doped in the catalyst layer. Although the COD removal rate is high, the service life is greatly reduced. In comparison between Example 3 and Example 2, only a high content of ruthenium is doped in the catalyst layer. Although the service life is long, the COD removal rate is poor.
[0118] according to Figure 1 The scanning electron microscope (SEM) characterization results show that the surface of the undoped metal titanium-based tin antimony anode presents a typical cracked mud structure. This structure is mainly due to the difference in thermal expansion coefficients between the active coating and the titanium substrate, as well as the uneven surface tension generated during the solvent drying process. After being doped with ruthenium or nickel alone, this cracked mud structure has improved, but it has not been completely resolved. After doping nickel and ruthenium at the same time in the titanium-based tin antimony anode, the cracked mud structure is significantly eliminated, the surface morphology becomes denser, and the stability and service life of the electrode are greatly improved.
[0119] according to Figure 2 The linear voltammetric sweep (LSV) characterization results show that the oxygen evolution potential of the bimetallic doped electrode is significantly improved compared with the undoped and single metal doped electrodes, the oxygen evolution side reaction is effectively inhibited, and the catalytic degradation activity of the electrode for organic matter is improved.
[0120] according to Figure 3 The electrochemically active area (ECSA) characterization results showed that the NiRu bimetallic doped electrode exhibited a higher electrochemically active area and an increased number of reaction sites, which was beneficial to improving the catalytic activity of the electrode.
[0121] according to Figure 4 The electrochemical impedance spectroscopy (EIS) characterization results show that the electrode doped with nickel-ruthenium bimetallic exhibits a lower charge transfer resistance, indicating that the charge transfer efficiency of the electrode has been significantly improved. The lower oxygen evolution potential, increased electrochemical active area, and lower charge transfer resistance all lead to higher performance of the electrode in the degradation of organic matter.
[0122] It should be noted that the LSV test conditions are as follows: the instrument model used: BiologicSP-150 electrochemical workstation from Bio-Logic, France; reference electrode: Ag / saturated AgCl electrode; counter electrode: Pt electrode; working electrode: prepared electrode; electrolyte: 0.05 mol·L -1 Sodium sulfate solution, scan rate 10 mV / s, potential window 1-3.2 V vs. RHE.
[0123] ECSA was obtained by cyclic voltammetry (CV) testing. The CV test conditions were as follows: the instrument model used was the Biologic SP-150 electrochemical workstation from Bio-Logic, France; the reference electrode was an Ag / saturated AgCl electrode; the counter electrode was a Pt electrode; the working electrode was the prepared electrode; the electrolyte was 0.05 mol·L -1 Sodium sulfate solution, scan rates were 20, 40, 60, 80, 100, 120 mV / s, potential window was 0.95-1.05 V vs. RHE.
[0124] EIS test conditions: Instrument model: Biologic SP-150 electrochemical workstation from Bio-Logic, France; reference electrode: Ag / saturated AgCl electrode; counter electrode: Pt electrode; working electrode: prepared electrode; electrolyte: 0.05 mol·L -1 Sodium sulfate solution, test frequency is 10 -2 -10 6 Hz, with an amplitude of 5mV.
Claims
1. A titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode, characterized in that: include: A titanium-containing substrate material and a catalyst supported on the substrate material; The catalyst includes nickel and ruthenium; The molar ratio of nickel to ruthenium is 1-4:1-4.
2. The titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode according to claim 1, characterized in that: The catalyst also includes tin and antimony, and the molar ratio of tin, antimony, nickel and ruthenium is 120-240:6-10:1-4:1-4.
3. The titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode according to claim 2, characterized in that: The catalyst loading on the substrate material is 1.2 to 3.0 mg / cm 2 .
4. The titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode according to any one of claims 1 to 3, characterized in that: The catalyst supported on the base material forms a catalytic layer.
5. A method for preparing a titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: S1, substrate pretreatment: grinding and etching the substrate material to obtain a pretreated substrate material; S2, precursor liquid coating: evenly apply the precursor liquid containing nickel and ruthenium to the pretreated substrate material; S3, drying and fixing: drying the coated substrate material; S4, calcining: calcining the dried base material; Wherein, the steps S2 to S4 are repeated N times to obtain a titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode; In the step S2, the molar ratio of nickel to ruthenium in the precursor solution is 1-4:1-4.
6. The method for preparing the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode according to claim 5, characterized in that: The precursor solution also contains tin and antimony, and the molar ratio of tin, antimony, nickel and ruthenium is 120-240:6-10:1-4:1-4.
7. The method for preparing the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode according to claim 5 or 6, characterized in that: In step S4, the calcination temperature is 400-700°C and the calcination time is 5-240 minutes; and / or The value of N is 10 to 20; in the first N-1 times of step S4, the calcination temperature is 400 to 700° C. and the time is 5 to 20 min; In the Nth step S4, the calcination temperature is 400-700° C. and the calcination time is 1-4 hours.
8. The method for preparing the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode according to claim 7, characterized in that: In the step S1, the etching process is to perform acid etching on the polished base material using an acid solution; and / or The acid for the acid etching treatment is one, two or more of oxalic acid, nitric acid, hydrochloric acid and sulfuric acid.
9. The method for preparing the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode according to claim 8, characterized in that: In step S3, the drying process is carried out at a temperature of 80 to 95° C. and for a time of 5 to 20 minutes.
10. Use of the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode as claimed in any one of claims 1 to 4, or the titanium-based nickel-ruthenium bimetallic doped tin-antimony electrode prepared by the method of any one of claims 5 to 9, in treating wastewater.
Citation Information
Patent Citations
Ni-doped tin dioxide microporous anode, preparation method and application
CN106395999A
Ru-doped electrode and application in electrocatalytic degradation of rhodamine B thereof
CN109851004A
Titanium-based tin antimony nickel metal coating electrode and preparation method and application thereof
CN115613070A
Technological method for treating carbolic acid waste water by electrochemical oxidation
CN1935679A
Composite oxide coating electrode for organic pollutant degradation, and preparation method therefor
WO2023088398A1
Cited By
Ru-Co co-doped Ti / SnO2-Sb anode and preparation method and application thereof
CN120903648A