Flow electrode capacitive device, system, preparation and application

By designing a mesh runner in a flow electrode capacitance device and optimizing the runner structure, the problem of low charge transfer and ion trapping efficiency in traditional devices is solved, and more efficient charge transfer and ion trapping are achieved, reducing flow resistance and Electrode accumulation.

CN118908367AActive Publication Date: 2024-11-08CENT SOUTH UNIV +1

Patent Information

Application Number
CN202410880723.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-08
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The traditional flow electrode capacitance device has low charge transfer and ion trapping efficiency, resulting in large flow resistance of the electrode slurry, electrode accumulation and runner blockage.

Method used

A flow electrode capacitance device including a mesh flow channel is designed. By optimizing the angle and length of the flow channel, a dispersible flow field with cross-linking and interoperable flow rate is formed, the flow resistance of the electrode slurry is reduced, and the electrode particles are evenly distributed, and the charge is enhanced. Transfer and ion trapping efficiency.

Benefits of technology

It effectively reduces the flow resistance of the electrode slurry, avoids particle aggregation and settlement, strengthens the charge transfer process and ion trapping efficiency, and improves the efficiency of seawater desalination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908367A_ABST
    Figure CN118908367A_ABST
Patent Text Reader

Abstract

The invention provides a flowing electrode capacitor device, a flowing electrode capacitor system, preparation and application. The flowing electrode capacitor device comprises a first current collector, a cation exchange membrane, a liquid inlet partition plate, an anion exchange membrane and a second current collector which are arranged in sequence. The working surfaces of the first current collector and the second current collector are respectively provided with a first flow channel and a second flow channel, and at least one of the first flow channel and the second flow channel is a net-shaped flow channel. The netted flow channels of the first current collector and the second current collector are cross-linked and intercommunicated dispersive flow channels, and the included angles and the lengths of the flow channels are optimized, so that a dispersive flow field generated by the cross-linked and intercommunicated flow channels can effectively reduce the flow resistance of electrode slurry, electrode particles are uniformly distributed in the flow channels, and the flow resistance of the electrode slurry is improved. The continuous aggregation or sedimentation process of particles in the flow channel is avoided, electron conduction is facilitated to expand to the central area of the flow channel, and the charge transfer process and the ion trapping efficiency of electrode slurry are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrically driven capacitors, and in particular to mobile electrode capacitor devices, systems, preparation and applications. Background Art

[0002] Treatment of high-salinity wastewater remains a serious challenge to the growing demand for fresh water, which has led to the development of various desalination technologies. Electrically driven capacitive deionization has low energy consumption and environmental friendliness, making it a promising technology for high-salinity wastewater treatment and seawater desalination. Flow-electrode capacitive deionization (FCDI) utilizes flowing electrode slurry and has a theoretically pseudo-infinite desalination capacity and can operate for a long time without the need for additional regeneration steps. Compared with reverse osmosis and multi-stage evaporation, FCDI further reduces energy consumption and improves the efficiency of seawater desalination.

[0003] The flow channel structure in FCDI devices has been shown to enhance the fluidity of electrode slurry. However, the charge transfer process and ion capture efficiency of traditional FCDI devices are low. Summary of the invention

[0004] The main purpose of the present invention is to provide a mobile electrode capacitor device, system, preparation and application to solve the technical problems of low charge transfer process and ion capture efficiency of traditional FCDI devices.

[0005] To achieve the above object, the present invention provides a mobile electrode capacitor device, comprising a first current collector, a cation exchange membrane, a liquid inlet partition, an anion exchange membrane and a second current collector arranged in sequence.

[0006] The working surfaces of the first current collector and the second current collector respectively have a first flow channel and a second flow channel, at least one of the first flow channel and the second flow channel is a mesh flow channel. The working surface is the surface of the first current collector and the second current collector facing the liquid inlet partition.

[0007] The mesh flow channel includes multiple grid units, in each of the grid units, the angle between any two adjacent flow channel edges is greater than 90°, the depth of the flow channel edge is 1 to 3 mm, and the width is 1 to 4 mm. The flow channel area corresponding to the total length of the mesh flow channel is 11.38 to 22.22% of the total area of ​​the working surface.

[0008] According to an embodiment of the present application, among the plurality of grid units, at least some of the grid units are the same, and their outlines are all regular polygons, and the number of side lengths of the regular polygons is 5-6.

[0009] According to an embodiment of the present application, the mesh flow channel includes a flow channel frame, and the mesh flow channel is arranged in an area surrounded by the flow channel frame and is connected to all frames of the flow channel frame.

[0010] According to an embodiment of the present application, a row of the grid units of the transverse frame close to the flow channel frame are all connected to the transverse frame through the end portions.

[0011] A row of the grid units of the vertical frame close to the flow channel frame are closely connected with the vertical frame through the flow channel edge.

[0012] According to an embodiment of the present application, the first current collector and the second current collector each include a liquid inlet and a liquid outlet communicated with the flow channel frame.

[0013] According to an embodiment of the present application, the depth of the solution cavity of the liquid inlet partition is 1 to 4 mm.

[0014] The projections of the first flow channel and the second flow channel on the liquid inlet partition along the thickness direction of the flow electrode capacitor device are both located in the solution cavity.

[0015] According to an embodiment of the present application, it also includes two end plates, two flexible gaskets and fasteners, and the end plate, the flexible gasket, the first current collector, the cation exchange membrane, the liquid inlet partition, the anion exchange membrane, the second current collector, the other flexible gasket and the end plate are arranged in sequence and fixed by the fasteners.

[0016] The present application also provides a flowing electrode capacitor system, comprising the flowing electrode capacitor device described above, a first delivery pump, a second delivery pump, a third delivery pump, electrode slurry and a power supply.

[0017] The first delivery pump and the first current collector form a first circulation channel, the second delivery pump and the second current collector form a second circulation channel, and the third delivery pump and the liquid inlet partition form a third circulation channel.

[0018] The electrode slurry is located in the first circulation channel and the second circulation channel, and the electrode slurry includes activated carbon, carbon nanotubes, carbon black and sodium chloride, the activated carbon accounts for 5-20% of the mass of the electrode slurry, the carbon nanotubes account for 0.1-1% of the mass of the electrode slurry, the carbon black accounts for 0.1-1% of the mass of the electrode slurry; the sodium chloride accounts for 0.1-2% of the mass of the electrode slurry.

[0019] The positive electrode of the power source is connected to the first current collector, and the negative electrode is connected to the second current collector.

[0020] The present application also provides a method for preparing a mobile electrode capacitor system, comprising the following steps:

[0021] The carbon nanotubes and conductive carbon black are mixed in a ratio of 1:1 to obtain a conductive additive.

[0022] The activated carbon and 1000 mg / L sodium chloride solution were mixed at a mass ratio of 2.5 to 20:100, and a conductive additive was added at a solid-liquid ratio of 0.2 to 2 g:100 ml, and stirred for 12 hours to obtain an electrode slurry.

[0023] The electrode slurry was ultrasonically dispersed for 30 minutes and then introduced into the above-mentioned flow electrode capacitor device.

[0024] The present application also provides an application of the above-mentioned mobile electrode capacitor system in water treatment, comprising the following steps:

[0025] The water to be treated is introduced into the solution cavity of the liquid inlet partition plate and circulated through the third delivery pump.

[0026] The electrode slurry is introduced into the first flow channel of the first current collector and circulated through the first delivery pump.

[0027] The electrode slurry is introduced into the second flow channel of the second current collector and circulated through the second delivery pump.

[0028] The first current collector and the second current collector are subjected to a preset electric field for 60 to 1800 minutes to perform desalination.

[0029] In the above-mentioned flowing electrode capacitor device, the mesh flow channels of the first current collector and the second current collector are cross-linked and interconnected dispersed flow channels, and the angle and length of the flow channels are optimized. The dispersed flow field generated by the cross-linked and interconnected flow channels can effectively reduce the flow resistance of the electrode slurry, make the electrode particles evenly distributed in the flow channel, avoid the continuous aggregation or sedimentation process of the particles in the flow channel, and facilitate the expansion of electron conduction to the central area of ​​the flow channel, thereby enhancing the charge transfer process of the electrode slurry and the ion capture efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0031] Figure 1 It is a structural schematic diagram of the mobile electrode capacitive deionization device in the present invention;

[0032] Figure 2 It is a schematic diagram of the structure of the mobile electrode capacitive deionization device in the present invention;

[0033] Figure 3 Flow channel structures of different types of graphite plates in the present invention, wherein (a) is a rectangular cavity (RC), (b) is a serpentine flow channel (SS), and (c) is a hexagonal honeycomb flow channel (HH);

[0034] Figure 4 It is a schematic diagram of the structure of the hexagonal honeycomb flow channel in the present invention;

[0035] Figure 5 Desalination performance of different types of flow channels in FCDI process in Example 1 of the present invention, including (a) brine concentration change, (b) induced voltage, (c) SR and ASRR, (d) CE and ENRS;

[0036] Figure 6 Desalination performance of different types of flow channels in Example 2 of the present invention under electrode slurry conditions with different carbon contents, including: (a) change in brine concentration of RC-FCDI system, (b) change in brine concentration of SS-FCDI system, (c) change in brine concentration of HH-FCDI system, (d) SR parameters of three FCDI systems, (f) ASRR parameters of three FCDI systems, (e) CE parameters of three FCDI systems;

[0037] Figure 7 The effects of different flow rates on the performance of the HH-FCDI system in Example 3 of the present invention: (a) brine concentration change, (b) induced voltage, (c) SR and average voltage, (d) ASRR and ENRS;

[0038] Figure 8 The effects of different initial concentrations on the performance of the HH-FCDI system in Example 4 of the present invention: (a) brine concentration change, (b) induced voltage, (c) SR and average voltage, (d) ASRR and ENRS;

[0039] Fig. 9 (a) particle migration mechanism, (b) CFD results and (c) FCDI long-term operating performance of the rectangular channel FCDI system in Example 5 of the present invention;

[0040] Fig.10 (a) particle migration mechanism, (b) CFD results and (c) FCDI long-term operating performance of the serpentine flow channel FCDI system in Example 5 of the present invention;

[0041] Fig.11 (a) particle migration mechanism of the hexagonal honeycomb flow channel FCDI system in Example 5 of the present invention,

[0042] (b) CFD results and (c) FCDI long-term operating performance.

[0043] 100, first current collector; 200, cation exchange membrane; 300, liquid inlet partition; 400, anion exchange membrane; 500, second current collector; 600, mesh flow channel; 610, grid unit; 611, flow channel edge;

[0044] 700, flow channel frame; 710, horizontal frame; 720, vertical frame; 800, end plate; 900, flexible gasket;

[0045] 1000. Fasteners;

[0046] 10. Flow electrode capacitor device; 21. First delivery pump; 22. Second delivery pump; 23. Third delivery pump; 50. Power supply; 60. Magnetic stirrer; 80. Electrode slurry storage tank; 90. Brine storage tank; 30. Computer control terminal.

[0047] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0050] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0051] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0052] The applicant has conducted extensive research on the technical problems of low charge transfer process and ion capture efficiency of traditional FCDI devices. The research found that most traditional FCDI devices are single-track serpentine flow channels. The single-track serpentine flow channel will produce a large flow resistance at the bend, causing excessive local hydraulic pressure, resulting in overflow of electrode slurry from the flow channel, causing serious electrode accumulation and flow channel blockage problems. Based on the two-phase flow characteristics of the electrode slurry, that is, the distribution (aggregation or dispersion) of the electrode particles is subject to the fluid dynamics behavior of the liquid electrolyte, and the flow channel structure dominates the flow state of the liquid electrolyte. Therefore, the flow channel structure can play a role in fluid guidance and electron supply in the FCDI process, which is crucial to the fluidity of the electrode slurry, particle migration and the construction of the charge conduction network.

[0053] On this basis, the present invention provides a mobile electrode capacitor device 10, see Figure 1 and Figure 4 , comprising a first current collector 100, a cation exchange membrane 200, a liquid inlet partition 300, an anion exchange membrane 400 and a second current collector 500 arranged in sequence. The working surfaces of the first current collector 100 and the second current collector 500 have a first flow channel and a second flow channel respectively.

[0054] The first current collector 100, the cation exchange membrane 200, the liquid inlet partition 300, the anion exchange membrane 400 and the second current collector 500 are closely attached, such as being fixed together by a fastener 1000. The surfaces of the first current collector 100 and the second current collector 500 facing the liquid inlet partition 300 are called working surfaces.

[0055] The materials of the first current collector 100 and the second current collector 500 are not specifically limited, and include various materials, such as a graphite plate structure. The first current collector 100 and the second current collector 500 are mechanically etched or chemically etched as needed to form grooves of corresponding shapes on the working surface to obtain corresponding first and second flow channels.

[0056] The cation exchange membrane 200 is closely attached to the working surface of the first current collector 100, and cooperates with the first flow channel to form a chamber for constraining the flow of the electrode slurry. The anion exchange membrane 400 is closely attached to the working surface of the second current collector 500, and cooperates with the second flow channel to form another chamber for constraining the flow of the electrode slurry. The two chambers are independent of each other.

[0057] The liquid inlet partition 300 has a receiving cavity, and the receiving cavity of the liquid inlet partition 300 is through in the thickness direction, that is, one side is in contact with the anion exchange membrane 400, and the other side is in contact with the cation exchange membrane 200. That is, the liquid inlet partition 300 is a hollow structure, providing a chamber for the flow of treated water. Therefore, in general, the mobile electrode capacitor device 10 includes a three-chamber structure arranged in sequence along the stacking direction.

[0058] At least one of the first flow channel and the second flow channel is a mesh flow channel 600 (also referred to as a distributed flow channel structure). The mesh flow channel 600 includes a plurality of grid units 610, wherein in each of the grid units 610, the angle between any two adjacent flow channel edges 611 is greater than 90°, the depth of the flow channel edge 611 is 1 to 3 mm, and the width is 1 to 4 mm, and the total length of the mesh flow channel 600 corresponds to a flow channel area of ​​11.38 to 22.22% of the total area of ​​the working surface.

[0059] See also Figure 1 and Figure 4 , the mesh flow channel 600 includes a plurality of grid units 610. The plurality of grid units 610 are arranged in multiple rows and columns, and are arranged and combined to form the mesh flow channel 600. Each grid unit 610 includes a plurality of flow channel edges 611, such as 5, 6, 7, 10, etc. flow channel edges 611, and all flow channel edges 611 are connected end to end to form the grid unit 610. Two adjacent grid units 610 share a portion of the flow channel edges 611, such as sharing one flow channel edge 611.

[0060] The types of the grid units 610 in the mesh flow channel 600 include one or more types. For example, all the grid units 610 are hexagonal grid units 610 with six flow channel edges 611 , and all the grid units 610 are pentagonal grid units 610 with five flow channel edges 611 .

[0061] Exemplarily, all grid units 610 include both hexagonal grid units 610 and pentagonal grid units 610. When the types of grid units 610 in the mesh flow channel 600 include multiple types, the number of different types of grid units 610 is not required to be the same, and they can be arranged as needed.

[0062] Regardless of the above-mentioned grid unit 610, in a single grid unit 610, the angle between any two adjacent flow channel edges 611 is greater than 90°, and the depth of the flow channel edge 611 is 1 to 3 mm, and the width is 1 to 4 mm. When the angle between any two adjacent flow channel edges 611 is greater than 90°, the electrode slurry encounters less resistance when flowing from one flow channel edge 611 to the adjacent flow channel edge 611.

[0063] The total length of the mesh flow channel 600 is the sum of the length of the flow channel edge 611 of all grid units 610 and the length of other flow channel parts except the grid units 610. The product of the total length of the mesh flow channel 600 and the width of the flow channel edge 611 is the flow channel area corresponding to the mesh flow channel 600. The flow channel area corresponding to the total length of the mesh flow channel 600 is 11.38-22.22% of the total area of ​​the working surface, ensuring that the total length of the mesh flow channel 600 is as long as possible, increasing the capacity of the electrode slurry in the mesh flow channel 600, and enhancing the processing capacity.

[0064] In the above-mentioned mobile electrode capacitor device 10, the mesh flow channels 600 of the first current collector 100 and the second current collector 500 are cross-linked and interconnected dispersed flow channels, and the angle and length of the flow channels are optimized. The dispersed flow field generated by the cross-linked and interconnected flow channels can effectively reduce the flow resistance of the electrode slurry, make the electrode particles evenly distributed in the flow channel, avoid the continuous aggregation or sedimentation process of the particles in the flow channel, and facilitate the expansion of electron conduction to the central area of ​​the flow channel, thereby enhancing the charge transfer process and ion capture efficiency of the electrode slurry.

[0065] In some embodiments, see Figure 4 Among the plurality of grid units 610, at least some of the grid units 610 are the same, and their outlines are all regular polygons, and the number of sides of the regular polygons is 5 to 6. In this case, the grid units 610 have regular shapes and are easy to etch and manufacture.

[0066] Exemplarily, the number of sides of the regular polygon is 6. The mesh flow channel 600 is a hexagonal honeycomb flow channel structure. The hexagonal honeycomb flow channel constructs a cross-linked and interconnected flow channel, which can efficiently divert and guide the electrode slurry, greatly reducing the flow resistance of the electrode slurry and ensuring its fluidity. The fluidity optimization caused by the flow channel structure can inhibit excessive accumulation or sedimentation of electrode particles, facilitate the dynamic aggregation of electrode particles and build a charge penetration network, thereby strengthening its charge transfer.

[0067] Specifically, the flow channel structure is supported by graphite plate carving. The flow channel area is arranged in a honeycomb shape by hexagons of the same size. The intervals between the hexagons are the flow channels of the electrode slurry. The flow channel depth is set to 2mm, and the flow channel area is 50×40mm, with an effective area of ​​10.24-20cm 2 , the corresponding total flow channel length is 512mm, and the effective flow channel volume is 2.04~4cm 3 .

[0068] Of course, in some embodiments, the outline of the grid unit 610 may also be a non-regular polygon.

[0069] In some embodiments, the mesh flow channel 600 includes a flow channel edge 611 frame, and the mesh flow channel 600 is disposed in an area surrounded by the flow channel edge 611 frame and is connected to all borders of the flow channel edge 611 frame.

[0070] With this arrangement, the flow channels in the mesh flow channel 600 are more abundant, and there are more inlets for the electrode slurry to enter the flow channel edge 611 frame, thereby reducing the congestion of the electrode slurry entering the flow channel edge 611 frame.

[0071] In some embodiments, a row of the grid units 610 near the horizontal frame 710 of the flow channel edge 611 is connected to the horizontal frame 710 through the end. A column of the grid units 610 near the vertical frame 720 of the flow channel edge 611 is closely connected to the vertical frame 720 through the flow channel edge 611.

[0072] The end of the grid unit 610 is the intersection of two adjacent flow channel edges 611 of the grid unit 610. A row of the grid units 610 close to the horizontal frame 710 framed by the flow channel edge 611 is connected to the horizontal frame 710 through a short flow channel.

[0073] A row of the grid units 610 of the vertical frame 720 close to the channel edge 611 are closely connected to the vertical frame 720 through the channel edge 611, such as the vertical frame 720 and the channel edge 611 are parallel and in contact, partially overlap, or do not overlap but only contact.

[0074] In some embodiments, the first current collector 100 and the second current collector 500 each include a liquid inlet and a liquid outlet connected to the flow channel edge 611. The electrode slurry enters from the liquid inlet and flows out from the liquid outlet.

[0075] In some embodiments, the depth of the solution cavity of the liquid inlet partition 300 is 1-4 mm. The projections of the first flow channel and the second flow channel along the thickness direction of the mobile electrode capacitor device 10 on the liquid inlet partition 300 are both located in the solution cavity.

[0076] The solution cavity of the liquid inlet partition 300 is a cavity penetrating in the thickness direction and having a depth of 1-4 mm, that is, one side contacts the anion exchange membrane 400 and the other side contacts the cation exchange membrane 200. Both the first flow channel and the second flow channel are within the scope of the solution cavity.

[0077] In some embodiments, it also includes two end plates 800, two flexible gaskets 900 and fasteners 1000, and the end plate 800, the flexible gasket 900, the first current collector 100, the cation exchange membrane 200, the liquid inlet partition 300, the anion exchange membrane 400, the second current collector 500, another flexible gasket 900 and the end plate 800 are arranged in sequence and fixedly connected by the fasteners 1000.

[0078] Exemplarily, the mobile electrode capacitor device 10 is sequentially composed of an acrylic end plate 800, a silicone gasket (flexible gasket 900), an anode graphite plate (first current collector 100), an anion exchange membrane 400, a brine compartment, a cation exchange membrane 200, a cathode graphite plate (second current collector 500), a silicone gasket (flexible gasket 900) and an end plate 800. The above components are assembled in series in a stacked manner by screws and nuts (fasteners 1000) to ensure the sealing of the FCDI device.

[0079] The present application also provides a flow electrode capacitor system, including the above-mentioned flow electrode capacitor device 10 (FCDI device), a first delivery pump 21, a second delivery pump 22, a third delivery pump 23, an electrode slurry and a power supply 50. The first delivery pump 21 and the first current collector 100 constitute a first circulation channel, the second delivery pump 22 and the second current collector 500 constitute a second circulation channel, and the third delivery pump 23 and the liquid inlet partition 300 constitute a third circulation channel. The specific structures of the first delivery pump 21, the second delivery pump 22, and the third delivery pump 23 are not limited, such as peristaltic pumps.

[0080] The electrode slurry is located in the first circulation channel and the second circulation channel. The electrode slurry includes activated carbon, carbon nanotubes, carbon black and sodium chloride. The activated carbon accounts for 5-20% of the mass of the electrode slurry, the carbon nanotubes account for 0.1-1% of the mass of the electrode slurry, and the carbon black accounts for 0.1-1% of the mass of the electrode slurry; the sodium chloride accounts for 0.1-2% of the mass of the electrode slurry. The activated carbon is used as a carrier for adsorbing target ions, and a high activated carbon content needs to be maintained; the carbon black, carbon nanotubes and sodium chloride electrolytes can effectively promote the formation of a conductive network in the slurry and improve the conductivity of the slurry, but their excessive content will cause the slurry fluidity to deteriorate and block the flow channel of the device. The positive electrode of the power supply 50 is connected to the first current collector 100, and the negative electrode is connected to the second current collector 500.

[0081] Taking the example of introducing salt water into the liquid inlet partition 300, the specific working principle is as follows:

[0082] The slurry is respectively transported to the anion / cation electrode chambers on both sides of the FCDI device by pumps, wherein the electrode chamber is composed of a graphite current collector with a flow channel etched therein, thereby providing a channel for the flow of the electrode slurry. In addition, the brine chamber is constructed by using anion / cation exchange membranes 200 and compartments, and can be used to isolate the electrode slurry from the brine. Under the action of an external electric field, the charged ions in the brine selectively pass through the ion exchange membrane into the electrode slurry and are stored in the double electric layer on the surface of the electrode particles, thereby completing the desalination process of the brine. At the same time, the two streams of electrode slurry after adsorbing anions / cations are pumped out of the outside of the FCDI device for mixed regeneration and then recycled.

[0083] The present application also provides a method for preparing a mobile electrode capacitor system, comprising the following steps:

[0084] The carbon nanotubes and conductive carbon black are mixed in a ratio of 1:1 to obtain a conductive additive.

[0085] The source of carbon nanotubes is LB120-50 purchased from Lion Corporation of Japan, and the source of conductive carbon black is EPC-600JD purchased from Lion Corporation of Japan.

[0086] The activated carbon and 1000 mg / L sodium chloride solution were mixed at a mass ratio of 2.5-20:100, and a conductive additive was added at a solid-liquid ratio of 0.2-2 g:100 ml, and stirred for 12 hours to obtain an electrode slurry.

[0087] The electrode slurry was ultrasonically dispersed for 30 minutes and then introduced into the above-mentioned flowing electrode capacitor device 10 .

[0088] For example, activated carbon, carbon nanotubes and carbon black are mixed with sodium chloride electrolyte and continuously stirred to ensure that the particles are completely wetted to obtain the ternary carbon composite flow electrode material. Before use, the slurry needs to be ultrasonically treated to disperse it.

[0089] Specifically, activated carbon and 1000 mg / L sodium chloride solution are mixed at a mass ratio of 2.5 to 20:100, and a conductive additive is added at a solid-liquid ratio of 0.2 to 2 g:100 ml, wherein the conductive additive is a mixture of carbon nanotubes and conductive carbon black at a ratio of 1:1. The electrode slurry needs to be stirred for 12 hours to ensure uniform mixing; the electrode slurry needs to be ultrasonically dispersed for 30 minutes before use to ensure its dispersibility.

[0090] The present application also provides an application of the above-mentioned mobile electrode capacitor system in water treatment, comprising the following steps:

[0091] The water to be treated is introduced into the solution chamber of the liquid inlet partition 300 and circulated through the third delivery pump 23 .

[0092] The electrode slurry is introduced into the first flow channel of the first current collector 100 and circulated by the first delivery pump 21 .

[0093] The electrode slurry is introduced into the second flow channel of the second current collector 500 and circulated by the second delivery pump 22 .

[0094] After the first current collector 100 and the second current collector 500 are subjected to a preset electric field for 60 to 1800 hours, desalination is performed.

[0095] Exemplarily, it includes the following steps:

[0096] S01, assembling the device components described in the mobile electrode capacitive deionization device in series by means of screws and nuts in a stacking manner, and arranging them in intervals in the order of an electrode chamber, a saline chamber, and an electrode chamber;

[0097] S02, pumping the electrode slurry and the brine into the water inlet of the FCDI device respectively by a peristaltic pump, so that they enter the corresponding chambers respectively and circulate in the FCDI device;

[0098] S03, after preset electric field parameters and reaction time, providing a pulse electric field to the current collector of the FCDI device to drive the FCDI device to desalinate.

[0099] like Figure 2 As shown, the FCDI system mainly includes a peristaltic pump, a conductivity meter, a FCDI electrode device, a magnetic stirrer 60, a power supply tester (power supply 50), an electrode slurry storage tank 80, a brine storage tank 90 and a computer control terminal 30. During operation, under the action of the peristaltic pump, the brine solution enters the FCDI device at a certain flow rate, and then keeps circulating between the brine storage tank and the FCDI device. For the electrode slurry, this study adopts a short-circuit closed operation mode, that is, under the action of the peristaltic pump, the electrode slurry enters the cathode chamber and the anode chamber respectively, and then the two slurries merge into the electrode slurry storage tank and keep circulating. The power supply 50 tester is used to apply an electric field to the FCDI device, and the changes in the induced current (I) or the induced voltage (V) are recorded in real time. In addition, the conductivity in the brine solution is monitored and recorded in real time by a conductivity meter connected to a computer. Without affecting the understanding of the present invention, in FCDI, C effluent concentration, C0 initial concentration, (C / C0) effluent concentration change, ASRR (μmol cm -2 min -1 ) Average desalination efficiency, CE (%), current efficiency, SR desalination efficiency (%), Em (kWh mol -1 ) Energy expenditure and ENRS (μmol J -1 ) Energy efficiency, used to evaluate desalination capacity.

[0100] In order to show the advantages of the special structure, three flow channel structures are set up, including rectangular cavity flow channel, single-serpentine flow channel and hexagonal-honeycomb flow channel, respectively referred to as RC-channel, SS-channel and HH-channel, and the corresponding FCDI units are RC-FCDI, SS-FCDI and HH-FCDI. The flow channel structures involved are all made of graphite plate carving, such as Figure 3 The channel depth is set to 2 mm, and the channel area is 50 × 40 mm. The effective areas of RC-channel, SS-channel and HH-channel are 20 cm 2 、10.88cm 2 and 10.99cm 2 , through calculation, the corresponding total lengths of the flow channels are 50mm, 544mm and 512mm respectively. Each FCDI electrode device (size: 90mm×80mm×7mm) is composed of an acrylic end plate, a graphite plate, an anion exchange membrane, a compartment, and a cation exchange membrane fixed by bolts. The effective area is the flow channel area for slurry flow, that is, the flow channel area corresponding to the total length of all flow channels; the flow channel area refers to the area of ​​the rectangular area due to the etching of the flow channel, that is, the area surrounded by the flow frame.

[0101] Based on the above embodiments, in order to facilitate understanding by those skilled in the art, examples are given below:

[0102] Example 1

[0103] The ternary carbon composite material was used as the electrode slurry, in which the mass fraction of activated carbon was 5.0wt.%, the mass fraction of carbon black + carbon nanotubes was 1.0wt.%, and the pulsed electric field parameters were set to have a pulse frequency of 5Hz, a duty cycle of 70%, and a pulse intensity of 90mA. The initial salt solution concentration was 7500mg L -1 (Conductivity is 12189μS cm -1 ). The FCDI desalination performance of three different types of flow channels was tested.

[0104] like Figure 5 As shown in Figure 2, the desalination performance of the three FCDI systems showed significant differences. Figure 5 (c) It can be seen that the HH-FCDI system has a high -1A higher SR (51.28%) was obtained in the brine, while that of the SS-FCDI and RC-FCDI systems was only 39.31 and 18.62%, respectively. Correspondingly, the HH-FCDI system exhibited a faster desalination rate, with an ASRR of 7.82 μmol cm -2 min -1 , which are 1.31 and 4.32 times of SS-FCDI and RC-FCDI systems respectively. Figure 5 (d) It can be seen that the CE of the HH-FCDI system (91.23%) is still better than that of RC-FCDI (76.69%) and SS-FCDI (85.51%), and the energy efficiency (ENRS) of the system reaches 15.31 μmol J -1 , which is significantly higher than RC-FCDI (11.16 μmol J -1 ) and SS-FCDI (12.72 μmol J -1 ), indicating that the HH-FCDI system exhibits excellent ion trapping efficiency.

[0105] Example 2

[0106] The ternary carbon composite material was used as the electrode slurry, in which different activated carbon mass fractions (2.5, 5.0, 12.5 and 20 wt.%) were set, the mass fraction of carbon black + carbon nanotubes was 1.0 wt.%, and the pulsed electric field parameters were set, the pulse frequency was 5 Hz, the duty cycle was 70%, the pulse intensity was 90 mA, and the initial salt solution concentration was 7500 mg L -1 (Conductivity is 12189μS cm -1 ). The desalination performance of FCDI under different carbon loadings was tested.

[0107] like Figure 6 As shown in Figure 2, with the increase of carbon loading, the effluent concentration (C / C0) of RC-FCDI and HH-FCDI systems continued to decrease, and when the carbon loading was 20 wt.%, the SR of the system reached the maximum, which was 45.47 and 63.42%, respectively, and the corresponding ASRR reached 3.95 and 9.45 μmol cm -2 min -1 For SS-FCDI, when the carbon loading increases from 12.5 to 20 wt.%, the SR and ASRR of the system decrease significantly, reaching only 41.63% and 6.37 μmol cm, respectively. -2 min -1 .

[0108] Too high a loading (20wt.%) will cause a sharp increase in the viscosity of the electrode slurry, and under the action of narrow continuous bends, the fluidity of the electrode slurry in the SS-FCDI system is further weakened, resulting in a large number of electrode particles being retained in the flow channel and blocked, which will seriously affect the ion capture efficiency of the system. The cross-linked and interconnected honeycomb flow channels in the HH-FCDI system can guide and divert the electrode slurry, which can effectively alleviate the weakening of fluidity caused by the excessively high viscosity of the electrode slurry and improve the flow efficiency of the electrode slurry.

[0109] In addition, when the loading amount increases from 12.5 to 20wt.%, the change trend of SR and ASRR in the HH-FCDI system is alleviated, and the CE of the system is significantly reduced, indicating that too high carbon loading will seriously weaken the fluidity of the electrode slurry. Based on the above analysis, we will use the electrode slurry with a carbon loading of 12.5wt.% for the next step.

[0110] Example 3

[0111] The ternary carbon composite material was used as the electrode slurry, in which the mass fraction of activated carbon was 12.5wt.%, the mass fraction of carbon black + carbon nanotubes was 1.0wt.%, and the pulsed electric field parameters were set to have a pulse frequency of 5Hz, a duty cycle of 70%, and a pulse intensity of 90mA. The initial salt solution concentration was 7500mg L -1 (Conductivity is 12189μS cm -1 ). Four different flow rates (V e =10, 25, 40 and 55mL min -1 ) to test the desalination performance of FCDI at different flow rates.

[0112] like Figure 7 As shown, when V e Increase from 10 to 40 mL min -1 When the effluent concentration (C / C0) of the HH-FCDI system continued to decrease, the desalination parameters were significantly improved, and at V e =40mL min -1 When , SR, ASRR and CE reached the highest values, which were 77.34%, 12.03 μmol cm -2 min -1 and 95.87%. The further improvement of HH-FCDI desalination performance indicates that the increase of flow rate promotes the fluidity of electrode slurry. e Further increase of V e =55mL min -1), the desalination performance decreased accordingly, among which SR, ASRR and CE decreased to 71.14%, 11.27 μmol cm -2 and 83.84%. Too high a flow rate will cause a sharp increase in pump energy consumption, which is not conducive to the practical application of the FCDI process. In order to pursue excellent desalination efficiency (i.e., SR, ASRR, and CE), this study will adopt V e =40mL min -1 Conduct follow-up experiments.

[0113] Example 4

[0114] Set different salt solution concentrations (C0 = 5, 7.5, 10 and 20 g L -1 ), the desalination performance of the HH-FCDI system under different initial salt concentration conditions was tested, and a ternary carbon composite material was used as the electrode slurry, in which the mass fraction of activated carbon was 12.5wt.%, the mass fraction of carbon black + carbon nanotubes was 1.0wt.%, and the pulsed electric field parameters were set, the pulse frequency was 5Hz, the duty cycle was 70%, and the pulse intensity was 90mA.

[0115] like Figure 8 As shown in Figure 2, with the increase of initial concentration, the effluent salt concentration curve (C / C0) gradually tends to be flat, and accordingly, the SR of the system continues to decrease, that is, from 98.68 (5.0 g L -1 ) decreased to 55.5% (10 g L -1 ). However, the ASRR increased significantly during the HH-FCDI process, from the initial 10.34 to 13.37 μmol cm -2 min -1 This indicates that the increase in salt ion concentration promotes the migration and diffusion of ions during FCDI. -1 ), CE decreased from 97.25 to 82.15%, and the energy efficiency ENRS of the system decreased from 28.88 to 23.3 μmol J -1 After comprehensive analysis, considering the negative impact of excessively high salt solution concentration, this study will select C0 = 10 g L -1 Conduct subsequent continuous desalination tests.

[0116] Example 5

[0117] Set the salt solution concentration C0 = 10 g L -1The desalination performance of the HH-FCDI system under different initial salt concentrations was tested. The ternary carbon composite material was used as the electrode slurry, in which the mass fraction of activated carbon was 12.5wt.%, the mass fraction of carbon black + carbon nanotubes was 1.0wt.%, and the pulsed electric field parameters were set. The pulse frequency was 5Hz, the duty cycle was 70%, the pulse intensity was 90mA, and the flow rate of the electrode slurry was set to 40mL min -1 And under the same conditions, RC-FCDI and SS-FCDI systems were set up for comparison.

[0118] like Figure 9-11 As shown in Figure 2, during the 1800-minute continuous operation of the RC-FCDI system, the effluent concentration change (C / C0) showed an obvious attenuation phenomenon. The final SR and CE of the system were only 26.62 and 76.44%, respectively. The average ASRR of the entire desalination process was 4.75 μmol cm -2 min -1 Compared with RC-FCDI, the SS-FCDI system exhibited better desalination performance, with the final SR and average ASRR reaching 50.71% and 8.07 μmol cm, respectively. -2 min -1 Compared with RC-FCDI and SS-FCDI systems, the HH-FCDI system showed more efficient and stable desalination performance in the continuous process. Specifically, the effluent salt concentration change (C / C0) was always stable at 0.082, and the final SR of the system reached 91.87%, that is, the concentration of the purified brine (C s ) decreased to 813.77 mg L -1 (Initial C s =10000mg L -1 ), and the average ASRR and CE of the entire run were 13.62 μmol cm -2 min -1 and 96.02%.

[0119] The present invention further optimizes the flow efficiency of the electrode slurry through the dispersed flow field generated by the honeycomb flow channel, promotes the charge conduction in the FCDI process, and thus realizes the efficient and stable continuous operation of the HH-FCDI system.

[0120] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A mobile electrode capacitor device, characterized in that: It includes a first current collector, a cation exchange membrane, a liquid inlet partition, an anion exchange membrane and a second current collector which are arranged in sequence; The working surfaces of the first current collector and the second current collector respectively have a first flow channel and a second flow channel, at least one of the first flow channel and the second flow channel is a mesh flow channel; the working surface is the surface of the first current collector and the second current collector facing the liquid inlet partition; The mesh flow channel includes multiple grid units, in each of the grid units, the angle between any two adjacent flow channel edges is greater than 90°, the depth of the flow channel edge is 1 to 3 mm, and the width is 1 to 4 mm. The flow channel area corresponding to the total length of the mesh flow channel is 11.38 to 22.22% of the total area of ​​the working surface.

2. The mobile electrode capacitor device according to claim 1, characterized in that: Among the plurality of grid units, at least some of the grid units are the same, and their outlines are all regular polygons, and the number of sides of the regular polygons is 5-6.

3. The mobile electrode capacitor device according to claim 1, characterized in that: The first flow channel and the second flow channel further include flow channel frames, and the mesh flow channel is arranged in a region surrounded by the flow channel frames and is in communication with all frames of the flow channel frames.

4. The mobile electrode capacitor device according to claim 3, characterized in that: A row of grid units close to the transverse frame of the flow channel frame are all connected to the transverse frame through the end portions; A row of the grid units of the vertical frame close to the flow channel frame are closely connected with the vertical frame through the flow channel edge.

5. The mobile electrode capacitor device according to claim 4, characterized in that: The first current collector and the second current collector each include a liquid inlet and a liquid outlet communicated with the flow channel frame.

6. The mobile electrode capacitor device according to any one of claims 1 to 5, characterized in that: The depth of the solution cavity of the liquid inlet partition is 1 to 3 mm; The projections of the first flow channel and the second flow channel on the liquid inlet partition along the thickness direction of the flow electrode capacitor device are both located in the solution cavity.

7. The mobile electrode capacitor device according to any one of claims 1 to 5, characterized in that: It also includes two end plates, two flexible gaskets and fasteners. The end plate, the flexible gasket, the first current collector, the cation exchange membrane, the liquid inlet partition, the anion exchange membrane, the second current collector, the other flexible gasket and the end plate are arranged in sequence and fixed by the fasteners.

8. A mobile electrode capacitance system, characterized in that: The mobile electrode capacitor device according to any one of claims 1 to 7, a first delivery pump, a second delivery pump, a third delivery pump, an electrode slurry and a power supply; The first delivery pump and the first current collector form a first circulation channel, the second delivery pump and the second current collector form a second circulation channel, and the third delivery pump and the liquid inlet partition form a third circulation channel; The electrode slurry is located in the first circulation channel and the second circulation channel, and the electrode slurry includes activated carbon, carbon nanotubes, carbon black and sodium chloride, wherein the activated carbon accounts for 5-20% of the mass of the electrode slurry, the carbon nanotubes account for 0.1-1% of the mass of the electrode slurry, the carbon black accounts for 0.1-1% of the mass of the electrode slurry; and the sodium chloride accounts for 0.1-2% of the mass of the electrode slurry; The positive electrode of the power source is connected to the first current collector, and the negative electrode is connected to the second current collector.

9. A method for preparing a mobile electrode capacitor system, characterized in that: The following steps are involved: The carbon nanotubes and the conductive carbon black are mixed in a ratio of 1:1 to obtain a conductive additive; The activated carbon and 1000 mg / L sodium chloride solution are mixed at a mass ratio of 2.5 to 20:100, and a conductive additive is added at a solid-liquid ratio of 0.2 to 2 g:100 ml, and stirred for 12 hours to obtain an electrode slurry; The electrode slurry is ultrasonically dispersed for 30 minutes and then introduced into the flowing electrode capacitor device as claimed in claim 8.

10. Application of the mobile electrode capacitor system according to claim 8 in water treatment, characterized in that: The following steps are involved: The water to be treated is introduced into the solution cavity of the liquid inlet partition plate and circulated through the third delivery pump; Introducing the electrode slurry into the first flow channel of the first current collector and circulating it through the first delivery pump; Introducing the electrode slurry into the second flow channel of the second current collector and circulating it through the second delivery pump; The first current collector and the second current collector are subjected to a preset electric field for 60 to 1800 minutes to perform desalination.

Citation Information

Patent Citations

  • Sea water desalination device and method for realizing desalination by utilizing alternated positive and negative adsorption

    CN108658179A

  • Capacitive desalination electrode material for mine water treatment and preparation method and application thereof

    CN115925062A

  • Continuous cation exchange membrane / solvent extraction / FCDI synergistic coupling lithium extraction method

    CN116497232A

  • Apparatus and corresponding method for purifying a fluid

    US20150315043A1

  • Method and apparatus for capacitive deionization and electrochemical purification and regeneration of electrodes

    US6309532B1

Cited By

  • Flow electrode continuous lithium extraction method and device based on Tesla runner

    CN122405972A