Flocculating agent and mud sludge dewatering and curing treatment process
By combining chitin, aspergillus fermentation broth and PLA-g-CS in the flocculant, an efficient flocculant is formed, which solves the problems of large amount of flocculant and pollution in the prior art, and achieves both strong flocculation effect and low pollution.
Patent Information
- Application Number
- CN202410998324.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
In the prior art, flocculants are difficult to take into account both high flocculation capacity and low pollution, especially the use of inorganic flocculants is large and easy to cause secondary pollution. When the use of organic flocculants is too large, it poses a threat to the environment and human health.
Using a flocculant, including chitin, Aspergillus fermentation broth, PLA-g-CS and epoxy quaternary ammonium salt, the floc is bound by hydrogen bonds, covalent bonds and coordination bonds, using Aspergillus niger and Aspergillus nitrite. The reaction of metabolic substances and chitosan forms a highly efficient flocculant and reduces contamination through biodegradable materials.
While achieving a strong flocculation effect, the accuracy of the dosage of flocculant is reduced, and the secondary pollution caused by the excessive use of epoxy quaternary ammonium salt is reduced. The flocculant is biodegradable and environmentally friendly.
Smart Images

Figure BDA0004960878720000071 
Figure BDA0004960878720000081 
Figure BDA0004960878720000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of mud sludge dehydration treatment, and more specifically, to a flocculant and a mud sludge dehydration solidification treatment process. Background Art
[0002] Silt is a kind of soft soil with flocculent or honeycomb structure formed by sedimentation in still water or slow-flowing water environment. Silt has high water content and many natural pores, so its mechanical strength is relatively poor. Mud is a mixture formed by silt diffused in water. The water content of mud is much greater than that of silt, that is, silt and mud have almost no strength. Silt and mud are difficult to prepare for engineering use. If they are directly abandoned, it will inevitably lead to a large waste of land resources.
[0003] At present, the dehydration and solidification process is usually used to treat sludge slurry, that is, flocculants are added to the sludge slurry, and then the sludge flocculants are dehydrated and solidified, so as to achieve the recycling of the sludge slurry. Among them, the flocculants can be mainly divided into inorganic flocculants or organic flocculants.
[0004] Common inorganic flocculants mainly include polyferric chloride, polyferric sulfate, polyaluminium chloride, polyaluminium sulfate, etc. However, the above inorganic flocculants are used in large amounts, and iron ions and aluminium ions can easily cause secondary pollution.
[0005] Common organic flocculants include polyacrylamide flocculants (PAM), cationic polyacrylamide flocculants (CPAM), etc. Although these organic flocculants have small dosages and strong flocculation ability, they have high dosage requirements. Once the above-mentioned organic flocculants are used in excessive amounts, the excess organic flocculants will easily cause harm to humans and the ecological environment.
[0006] Therefore, there is an urgent need for a flocculant and a mud sludge dehydration and solidification treatment process that has strong flocculation ability and is not prone to secondary pollution. Summary of the invention
[0007] In order to improve the defect of the flocculant in the prior art that it is difficult to achieve both high flocculation and low pollution, the present application provides a flocculant and a mud sludge dehydration and solidification treatment process.
[0008] In the first aspect, the present application provides a flocculant, which adopts the following technical solution: A flocculant comprises the following raw materials in parts by weight: 16-20 parts of chitin, 4-6 parts of Aspergillus fermentation broth, 2-3 parts of PLA-g-CS, 10-12 parts of epoxy quaternary ammonium salt and 8-12 parts of calcium salt, wherein the Aspergillus fermentation broth contains Aspergillus niger and Aspergillus nidulans, and the PLA-g-CS is prepared by grafting chitosan with carboxyl-terminated polylactic acid.
[0009] Through the above technical scheme, chitosan contains a large number of hydroxyl and amino groups, which can form hydrogen bonds, covalent bonds or coordination bonds with organic molecules in sludge, such as proteins, amino acids, nucleic acids, phenolic compounds, etc., and firmly combine to achieve the flocculation effect; moreover, chitosan is biodegradable, non-toxic and harmless, and is unlikely to cause secondary pollution to the environment.
[0010] There are living Aspergillus niger and Aspergillus nidulans in the Aspergillus fermentation broth. The living Aspergillus niger and Aspergillus nidulans reproduce in large numbers on the surface of PLA-g-CS with the help of PLA-g-CS as a carrier. Among them, there are some short hyphae on the surface of Aspergillus niger mycelial balls, and these short hyphae have an adsorption effect on small particles, causing the flocs to gradually gather around the PLA-g-CS.
[0011] In addition, as Aspergillus niger continues to grow and reproduce, the concentration of metabolites secreted by Aspergillus niger outside the cell is greater on the surface of PLA-g-CS than in other areas of the solvent; the extracellular substances produced by Aspergillus niger metabolism are mostly small molecules such as citric acid, gluconic acid, and oxalic acid. These extracellular substances have excellent flocculation effects, which further cause the flocculants to gradually accumulate around PLA-g-CS; and both Aspergillus niger fermentation broth and PLA-g-CS are biodegradable, and are unlikely to cause secondary pollution to the environment.
[0012] In addition to having excellent flocculation properties, Aspergillus nidulans in the Aspergillus fermentation broth can also form chitin deacetylase under the induction of chitosan in PLA-g-CS. The chitin deacetylase deacetylates part of the chitin, thereby embedding part of the chitin into PLA-g-CS.
[0013] Chitosan contains three types of active groups, namely C2-NH2, C3-OH, and C6-OH, among which C2-NH2 is a primary amino group with a lone pair of electrons and strong nucleophilicity; C3-OH is a secondary hydroxyl group and cannot rotate freely, has a large steric hindrance, and has poor activity; C6-OH is a primary hydroxyl group and can rotate freely in spatial conformation, has a small steric hindrance, and has a high activity; therefore, both C2-NH2 and C6-OH can react with the epoxy group in the epoxy quaternary ammonium salt, thereby introducing a quaternary ammonium salt group into the chitosan on PLA-g-CS, thereby effectively increasing the flocculation effect of PLA-g-CS, and then promoting the flocculant to obtain a stronger flocculation effect.
[0014] Due to the presence of chitosan, Aspergillus fermentation broth and PLA-g-CS, the amount of epoxy quaternary ammonium salt added is relatively small, which makes the flocculant have a larger addition range, effectively reduces the dosage accuracy of the flocculant, and thus reduces the possibility of secondary pollution caused by excessive epoxy quaternary ammonium salt.
[0015] Metal cations can enhance the bridging and charge neutralization effects of flocculants, thereby improving the flocculation effect of flocculants. Common metal cation additives include trivalent iron salts, trivalent aluminum salts and divalent calcium salts. However, compared with divalent calcium salts, trivalent iron salts and trivalent aluminum salts are prone to secondary pollution problems, so calcium salts are relatively better.
[0016] Preferably, the Aspergillus fermentation broth is a mixture of Aspergillus niger fermentation broth and Aspergillus nidulans fermentation broth, and the mass ratio of the Aspergillus niger fermentation broth to the Aspergillus nidulans fermentation broth is (3-5):1.
[0017] Through the above technical scheme, if the content of Aspergillus niger fermentation liquid is too low, the substances secreted by Aspergillus niger outside the cells are insufficient, thereby reducing the flocculation ability of the flocculant; if the content of Aspergillus niger fermentation liquid is too high, the substances secreted by Aspergillus niger outside the cells have sufficient flocculation effect, while the content of Aspergillus niger is low, thereby reducing the amount of chitin deacetylase generated, reducing the effect of embedding chitosan into PLA-g-CS, and thus reducing the flocculation effect of the flocculant; for this reason, the applicant finally determined, after a lot of research and experimental verification, that the mass ratio of Aspergillus niger fermentation liquid to Aspergillus nidulans fermentation liquid in the present application is preferably the above.
[0018] Preferably, the preparation method of PLA-g-CS comprises the following steps: Preparation of carboxyl-terminated polylactic acid: weigh lactide, water, and zinc lactate, mix them evenly, heat them under nitrogen protection to melt the reactants, and obtain carboxyl-terminated polylactic acid; Preparation of PLA-g-CS: dissolving the carboxyl-terminated polylactic acid in dimethyl sulfoxide, adding 1-ethyl-3-dimethylaminopropylcarbodiimide hydrochloride and N-hydroxysuccinimide, stirring at a constant temperature, adding chitosan solution to react, dialyzing to remove impurities, filtering to remove precipitates, and freeze-drying to obtain PLA-g-CS.
[0019] According to the technical scheme, zinc lactate is first used as a catalyst to initiate the ring-opening polymerization of lactide under molten conditions with water to obtain carboxyl-terminated polylactic acid; then 1-ethyl-3-dimethylaminopropylcarbodiimide hydrochloride and N-hydroxysuccinimide are used as catalysts to prepare PLA-g-CS by coupling reaction between the amino group in the CS molecule and the carboxyl group in the carboxyl-terminated polylactic acid.
[0020] Preferably, the mass ratio of the carboxyl-terminated polylactic acid to the chitosan in the chitosan solution is 10:(0.4-0.8).
[0021] Through the above technical scheme, if the content of chitosan is too high compared with that of terminal carboxyl polylactic acid, the self-polymerization reaction of chitosan may dominate, reducing the grafting rate of terminal carboxyl polylactic acid, thereby reducing the flocculation ability of the flocculant; if the content of chitosan is too low compared with that of terminal carboxyl polylactic acid, insufficient chitosan may be grafted onto the terminal carboxyl polylactic acid, which also reduces the flocculation ability of the flocculant; for this reason, the applicant finally determined, after a lot of research and experimental verification, that the mass ratio of carboxyl polylactic acid and chitosan in this application is preferably as mentioned above.
[0022] Preferably, the epoxy quaternary ammonium salt is a mixture of 2,3-epoxypropyl dodecyl dimethyl ammonium chloride and epoxypropyl trimethyl ammonium chloride.
[0023] Through the above technical scheme, both 2,3-epoxypropyl dodecyl dimethyl ammonium chloride and epoxypropyl trimethyl ammonium chloride have epoxy groups and quaternary ammonium salt groups, so both can react with chitosan; wherein, 2,3-epoxypropyl dodecyl dimethyl ammonium chloride has long chain branches, and epoxypropyl trimethyl ammonium chloride has short chain branches, thereby enabling PLA-g-CS to have a mixed structure of cations, long chain branches, and short chain branches, and further, when dehydrating the mud sludge, the flocculant can form large and dense sludge flocs, that is, the flocculant can have a better flocculation effect; and the obtained mud cake has a porous structure, thereby improving the compressibility of the mud cake and the filterability of water.
[0024] Preferably, the mass ratio of 2,3-epoxypropyldodecyldimethylammonium chloride to epoxypropyltrimethylammonium chloride is (1-3):1.
[0025] According to the above technical scheme, if the content of 2,3-epoxypropyl dodecyl dimethyl ammonium chloride is too little, the mixed structure of cations, long chain branches and short chain branches on the surface of PLA-g-CS will be dominated by short chain branches, and the overall structure will be imperfect, thereby reducing the flocculation ability of the flocculant; if the content of 2,3-epoxypropyl dodecyl dimethyl ammonium chloride is too high, the mixed structure of cations, long chain branches and short chain branches on the surface of PLA-g-CS will be dominated by long chain branches, and the overall structure will still be imperfect, which also reduces the flocculation ability of the flocculant; for this reason, the applicant finally determined that the mass ratio of 2,3-epoxypropyl dodecyl dimethyl ammonium chloride to epoxypropyl trimethyl ammonium chloride in this application is preferably as above after a lot of research and experimental verification.
[0026] In a second aspect, the present application provides a method for preparing a flocculant, which adopts the following technical solution: A method for preparing a flocculant, for preparing any of the above-mentioned flocculants, comprises the following steps: firstly, chitosan, Aspergillus fermentation broth and PLA-g-CS are added to a solvent and stirred sufficiently, then epoxy quaternary ammonium salt is added, and then stirred under UVA ultraviolet environment to finally obtain a flocculant.
[0027] Through the above technical scheme, the UVA ultraviolet environment can not only promote the simpler and more stable introduction of epoxy quaternary ammonium salts into chitosan, but also has extremely low inhibitory effect on Aspergillus. It can also induce mutations in the Aspergillus fermentation broth, thereby improving the stability of Aspergillus niger and Aspergillus nidulans in the Aspergillus fermentation broth, and indirectly improving the flocculation effect of the flocculant.
[0028] Preferably, when stirring under UVA ultraviolet environment, the reaction temperature is 35-40° C. and the reaction time is 8-10 h.
[0029] Through the above technical scheme, when the above reaction temperature and reaction time are adopted, the epoxy quaternary ammonium salt can be introduced into chitosan more simply and stably, and Aspergillus niger and Aspergillus nidulans in the Aspergillus fermentation broth can be more stable, which indirectly improves the flocculation effect of the flocculant.
[0030] Preferably, when stirring under UVA ultraviolet environment, the ultraviolet wavelength is 400-405nm and the pH value is 5-7.
[0031] Through the above technical scheme, when the above pH value and ultraviolet wavelength are used, the epoxy quaternary ammonium salt can be introduced into chitosan more simply and stably, and Aspergillus niger and Aspergillus nidulans in the Aspergillus fermentation broth can be more stable, which indirectly improves the flocculation effect of the flocculant.
[0032] In a third aspect, the present application provides a sludge dehydration and solidification treatment process, which adopts the following technical solution: A sludge dehydration and solidification treatment process comprises the following steps: Extraction: The sludge slurry is extracted into the sludge pool and then mixed and stirred evenly; Sedimentation: adding the above flocculants to the sludge slurry, followed by stirring, mixing and sedimentation to obtain stratified sludge floccules and supernatant liquid; Dehydration: Transfer the mud flocs to the geotextile for dehydration and filtration to obtain the solidified mud cake and take it out.
[0033] Through the above technical solution, when the above flocculant is added to the sludge slurry, over time, Aspergillus niger and Aspergillus nidulans gradually multiply in large quantities with PLA-g-CS as the carrier, the hyphae of Aspergillus niger begin to adsorb small particles, and the metabolic substances secreted by Aspergillus niger outside the cell gradually exert a flocculation effect. The chitin deacetylase formed by Aspergillus nidulans promotes the binding of chitin to PLA-g-CS. At the same time, chitin exerts a flocculation effect, and most of the mud gradually forms mud flocs with PLA-g-CS as the center, thereby completing solid-liquid separation.
[0034] In summary, this application has the following beneficial effects: 1. PLA-g-CS is used as a growth carrier for Aspergillus niger and Aspergillus nidulans in Aspergillus fermentation broth. In addition to having excellent flocculation performance, Aspergillus nidulans in Aspergillus fermentation broth can also form chitin deacetylase under the induction of soluble chitosan. Chitin deacetylase deacetylates part of chitin to form chitosan. Chitosan reacts with the epoxy group in the epoxy quaternary ammonium salt, thereby introducing quaternary ammonium salt groups at the chitosan on PLA-g-CS, thereby promoting the flocculant to obtain a stronger flocculation effect; and the flocculant has good biodegradability, reducing the pollution of the flocculant to the environment; 2. Chitosan, PLA-g-CS and Aspergillus fermentation broth are all non-toxic and harmless. Due to the presence of the three, the amount of epoxy quaternary ammonium salt added is relatively small, which makes the flocculant have a larger addition range, effectively reduces the dosage accuracy of the flocculant, and thus reduces the possibility of secondary pollution caused by excessive epoxy quaternary ammonium salt; 3. Epoxypropyltrimethylammonium chloride has short chain branches, and 2,3-epoxypropyldodecyldimethylammonium chloride has long chain branches, which makes PLA-g-CS have a mixed structure of cations, long chain branches, and short chain branches. When the mud sludge is dehydrated, the flocculant can form large and dense sludge flocs, that is, the flocculant can have a better flocculation effect. DETAILED DESCRIPTION
[0035] Raw materials chitin CAS: 1398-61-4; lactide CAS: 13076-17-0; chitosan CAS: 9012-76-4; epoxypropyl trimethyl ammonium chloride CAS: 3033-77-0; epichlorohydrin CAS: 106-89-8; ether CAS: 60-29-7; dodecyl dimethylamine CAS: 112-18-5; Aspergillus niger spore powder Ruiyuan 5 billion; Aspergillus nidulans spore powder Shanghai Yansheng; LB culture medium Kaiheng Biology; polyacrylamide flocculant Shouxin Environmental Protection CAS 9003-05-8; Different types of calcium salts can be selected. This application specifically uses calcium silicate with CAS number 1344-95-2 as an example for experiment. Calcium silicate also contains silicate ions, and silicate ions have extremely strong adsorption and bridging capabilities for colloidal particles in sludge slurry. The positively charged hydroxyl calcium ions obtained by hydrolysis of calcium salts, when the two are compounded, can both exert electrical neutralization capabilities and obtain adsorption and bridging capabilities, thereby further improving the flocculation effect of the flocculant.
[0036] 2,3-Epoxypropyl dodecyl dimethyl ammonium chloride: 40 kg of epichlorohydrin was added to 30 kg of ether, followed by dropwise addition of 27 kg of dodecyl dimethyl amine, followed by reaction at 20°C for 10 hours, and finally filtration, washing, and drying to obtain 2,3-epoxypropyl dodecyl dimethyl ammonium chloride.
[0037] Aspergillus niger fermentation broth: 0.1 g of Aspergillus niger spore powder was recovered and then inoculated into 100 ml of LB medium, and cultured in a shaking incubator at 28° C. for 72 h to obtain Aspergillus niger fermentation broth.
[0038] Aspergillus nidulans fermentation broth: 0.6 g of Aspergillus nidulans spore powder was recovered and then inoculated into 100 ml of LB medium, and cultured in a shaking incubator at 28° C. for 72 h to obtain Aspergillus nidulans fermentation broth.
[0039] The present application is further described in detail below in conjunction with embodiments and comparative examples. Example
[0040] Example 1 1. Preparation of PLA-g-CS 1. Preparation of carboxyl-terminated polylactic acid: Weigh 12.5 kg of lactide, 0.25 kg of water, and 0.1 kg of zinc lactate and add them into a polymerization tube. Heat at 140 ° C under nitrogen protection to melt the reactants. When all the liquid in the polymerization tube turns into a milky white solid, freeze the milky white solid with liquid nitrogen and dry it in a vacuum drying oven to obtain carboxyl-terminated polylactic acid. 2. Preparation of PLA-g-CS: 10 kg of carboxyl-terminated polylactic acid was dissolved in 60 L of dimethyl sulfoxide, 500 g of 1-ethyl-3-dimethylaminopropylcarbodiimide hydrochloride and 500 g of N-hydroxysuccinimide were added, and the mixture was stirred at 30°C for 1 h; 0.7 kg of soluble chitosan was added to 5 L of dimethyl sulfoxide to prepare a chitosan solution, the chitosan solution was added to the above solution and reacted for 4 h, impurities were removed by dialysis, the precipitate was removed by suction, and PLA-g-CS was obtained by freeze-drying.
[0041] 2. Preparation of flocculant First, 18 kg of chitosan, 5 kg of Aspergillus fermentation liquid and 2.5 kg of PLA-g-CS were mixed evenly at a stirring speed of 50 r / min for 6 hours; then, 11 kg of epoxy quaternary ammonium salt and 10 kg of calcium silicate were added to obtain a reaction solution; the reaction solution was reacted under a long-wave ultraviolet light environment of 403 nm; the reaction temperature was 38° C., the reaction time was 9 hours, and the reaction pH was adjusted to 6 with hydrochloric acid and sodium hydroxide.
[0042] The Aspergillus fermentation broth is a mixture of Aspergillus niger fermentation broth and Aspergillus nidulans fermentation broth, and the mass ratio of Aspergillus niger fermentation broth to Aspergillus nidulans fermentation broth is 4: 1. The epoxy quaternary ammonium salt is a mixture of 2,3-epoxypropyl dodecyl dimethyl ammonium chloride and epoxypropyl trimethyl ammonium chloride, and the mass ratio of 2,3-epoxypropyl dodecyl dimethyl ammonium chloride to epoxypropyl trimethyl ammonium chloride is 2: 1.
[0043] A sludge dehydration and solidification process comprises the following steps: Extraction: 100L of sludge slurry is extracted into the sludge pool, and then mixed and stirred evenly; Sedimentation: Add 5 kg of flocculant to the sludge slurry, then stir at a stirring speed of 100 r / min for 2 h, and then precipitate to obtain layered sludge flocs and supernatant; Dehydration: Transfer the mud flocs to the geotextile for dehydration and filtration to obtain the solidified mud cake and take it out.
[0044] Example 2-3 In Example 2-3, based on the preparation method of Example 1, the addition amount of each component of the flocculant was adjusted, and the specific adjustment is shown in Table 1.
[0045] Comparative Example 1-2 Comparative Example 1-2 is based on the preparation method of Example 1, and the addition amount of each component of the flocculant is adjusted. The specific adjustment is shown in Table 1.
[0046] Comparative Example 3 Comparative Example 3 is based on the preparation method of Example 1, except that the flocculant is replaced with polyacrylamide flocculant.
[0047] Table 1 Addition amount of each component of Examples 1-3 and Comparative Examples 1-2 (kg) project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Chitosan 18 16 20 18 18 Aspergillus fermentation broth 5 4 6 5 5 PLA-g-CS 2.5 2 3 3.5 1.5 Epoxy quaternary ammonium salt 11 12 10 11 11 Calcium silicate 10 8 12 10 10 Performance testing Flocculation effect and flocculation time test 100 ml of sludge slurry was mixed and stirred until uniform, and then 100 ml of sludge slurry was added to a 250 ml measuring cylinder. Every 3 measuring cylinders of sludge slurry were regarded as a group, and then 5 g of flocculant provided by the examples of the present application and the comparative example was added to each group of measuring cylinders, and then allowed to stand for 30 minutes to obtain sludge flocs and supernatant.
[0048] The mud flocculants were then filtered, dried and weighed. Finally, the average value of the data measured by the three measuring cylinders in each group was taken as the flocculation effect parameter and recorded. The results are shown in Table 2.
[0049] Record the time when the mud floccules reach the 20mL mark in the test tube. Finally, take the average value of the data measured by the three measuring cylinders in each group as the flocculation time parameter and record it. The results are shown in Table 2.
[0050] Table 2 Performance test table of Examples 1-3 and Comparative Examples 1-3 Referring to Table 2, by comparing Examples 1-3 and Comparative Examples 1-3, it can be seen that, relative to Example 1, the flocculation effect parameters of Examples 2-3 are decreased and the flocculation time is increased, while the flocculation effect parameters of Comparative Examples 1-2 are greatly decreased and the flocculation time is greatly increased. This indicates that the components of the flocculant have a better flocculation effect under the ratio of Example 1.
[0051] In addition, the flocculation effect of Examples 1-3 greatly exceeds that of Comparative Example 3, and the flocculation time of Examples 1-3 is greatly lower than that of Comparative Example 3, indicating that the flocculation ability of the flocculants prepared in Examples 1-3 exceeds that of the polyacrylamide flocculant.
[0052] Embodiment 4-5 In Example 4-5, based on the preparation method of Example 1, the mass ratio of the fermentation broth of Aspergillus niger to the fermentation broth of Aspergillus nidulans was adjusted, and the specific adjustment is shown in Table 3.
[0053] Comparative Examples 4-5 Comparative Example 4-5 Based on the preparation method of Example 1, the mass ratio of Aspergillus niger fermentation broth to Aspergillus nidulans fermentation broth was adjusted, and the specific adjustment is shown in Table 3.
[0054] The flocculants prepared in Example 4-5 and Comparative Example 4-5 were subjected to the above performance tests, and the test results are shown in Table 3.
[0055] Table 3 Addition amount and performance test data of Aspergillus niger fermentation broth and Aspergillus nidulans fermentation broth of Example 1, Example 4-5 and Comparative Example 4-5 Referring to Table 3, by comparing Example 1, Example 4-5 and Comparative Example 4-5, it can be seen that as the content of Aspergillus niger fermentation broth continues to increase, the flocculation effect and flocculation time of the flocculant first increase and then decrease. This may be because as the content of Aspergillus niger fermentation broth continues to increase, the substances secreted by Aspergillus niger outside the cell continue to increase, and the flocculation ability of the flocculant is continuously improved; however, if the content of Aspergillus niger fermentation broth is too high, the substances secreted by Aspergillus niger outside the cell already have sufficient flocculation effect, and the content of Aspergillus niger is low, which reduces the generation of chitin deacetylase, reduces the effect of embedding chitin into PLA-g-CS, and thus reduces the flocculation ability of the flocculant.
[0056] Embodiment 6-8 In Examples 6-8, based on the preparation method of Example 1, the mass ratio of carboxyl-terminated polylactic acid to chitosan in the chitosan solution was adjusted. The specific adjustment is shown in Table 4.
[0057] Comparative Examples 6-7 In Comparative Example 6-7, based on the preparation method of Example 1, the mass ratio of carboxyl-terminated polylactic acid to chitosan in the chitosan solution was adjusted, and the specific adjustment is shown in Table 4.
[0058] The flocculants prepared in Examples 6-8 and Comparative Examples 6-7 were subjected to the above performance tests, and the test results are shown in Table 4.
[0059] Table 4 Addition amount and performance test data of carboxyl-terminated polylactic acid and chitosan of Example 1, Examples 6-8 and Comparative Examples 6-7 Referring to Table 4, by comparing Example 1, Examples 6-8 and Comparative Examples 6-7, it can be seen that as the content of chitosan continues to increase, the flocculation effect and flocculation time of the flocculant first increase and then decrease. This may be because as the chitosan content continues to increase, chitosan is continuously grafted onto the carboxyl-terminated polylactic acid, continuously improving the flocculation ability of the flocculant; however, if the chitosan content is too high, the self-polymerization reaction of chitosan dominates, reducing the grafting rate of the carboxyl-terminated polylactic acid, thereby reducing the flocculation ability of the flocculant.
[0060] Examples 9-10 In Examples 9-10, based on the preparation method of Example 1, the mass ratio of 2,3-epoxypropyldodecyldimethylammonium chloride (referred to as "2,3-cyclic ammonium chloride" in the table) and epoxypropyltrimethylammonium chloride (referred to as "cyclic ammonium chloride" in the table) was adjusted, and the specific adjustment is shown in Table 5.
[0061] Comparative Examples 8-9 In Comparative Examples 8-9, based on the preparation method of Example 1, the mass ratio of 2,3-epoxypropyldodecyldimethylammonium chloride (referred to as "2,3-cyclic ammonium chloride" in the table) and epoxypropyltrimethylammonium chloride (referred to as "cyclic ammonium chloride" in the table) was adjusted, and the specific adjustment is shown in Table 5.
[0062] The flocculants prepared in Examples 9-10 and Comparative Examples 8-9 were subjected to the above performance tests, and the test results are shown in Table 5.
[0063] Table 5: Addition amount and performance test data of 2,3-cyclic ammonium chloride and cyclic ammonium chloride in Example 1, Examples 9-10 and Comparative Examples 8-9 Referring to Table 5, by comparing Example 1, Examples 9-10 and Comparative Examples 8-9, it can be seen that as the content of 2,3-epoxypropyldodecyldimethylammonium chloride continues to increase, the flocculation effect and flocculation time of the flocculant first increase and then decrease. This may be because as the chitosan content continues to increase, the mixed structure of cations, long branches and short branches on the surface of chitosan first continues to improve and then reaches a critical point, and then the mixed structure is dominated by short branches, which makes the flocculation ability of the flocculant continue to increase and then decrease.
[0064] Examples 11-12 In Examples 11-12, based on the preparation method of Example 1, the reaction temperature and reaction time during the preparation of the flocculant were adjusted. The specific adjustments are shown in Table 6.
[0065] Comparative Examples 10-11 In Comparative Examples 10-11, based on the preparation method of Example 1, the reaction temperature and reaction time during the preparation of the flocculant were adjusted. The specific adjustments are shown in Table 6.
[0066] The flocculants prepared in Examples 11-12 and Comparative Examples 10-11 were subjected to the above performance tests. The test results are shown in Table 7.
[0067] Table 6 Reaction conditions of Example 1, Examples 11-12 and Comparative Examples 10-11 project Reaction temperature / ℃ Reaction time / h Example 1 38 9 Embodiment 11 35 10 Example 12 40 8 Comparative Example 10 32 11 Comparative Example 11 45 7 Table 7 Performance test data of Example 1, Examples 11-12 and Comparative Examples 10-11 Referring to Table 7, by comparing Example 1, Examples 11-12 and Comparative Examples 10-11, it can be seen that, relative to Example 1, the flocculation effect parameters of Examples 11-12 are decreased and the flocculation time is increased, while the flocculation effect parameters of Comparative Examples 10-11 are greatly decreased and the flocculation time is greatly increased. This indicates that the components of the flocculant have a better flocculation effect under the ratio of Example 1.
[0068] Examples 13-16 In Examples 13-14, based on the preparation method of Example 1, the ultraviolet wavelength during the preparation of the flocculant was adjusted, and the specific adjustments are shown in Table 8.
[0069] In Examples 15-16, based on the preparation method of Example 1, the pH during the preparation of the flocculant was adjusted, and the specific adjustments are shown in Table 8.
[0070] Comparative Examples 12-15 In Comparative Examples 12-13, based on the preparation method of Example 1, the ultraviolet wavelength during the preparation of the flocculant was adjusted, and the specific adjustments are shown in Table 8.
[0071] In Comparative Examples 14-15, based on the preparation method of Example 1, the pH of the flocculant during preparation was adjusted, and the specific adjustments are shown in Table 8.
[0072] The flocculants prepared in Examples 13-16 and Comparative Examples 12-15 were subjected to the above performance tests. The test results are shown in Table 9.
[0073] Table 8 Reaction conditions of Example 1, Examples 13-16 and Comparative Examples 12-15 Table 9 Performance test data of Example 1, Examples 13-16 and Comparative Examples 12-15 Referring to Table 9, by comparing Example 1, Examples 13-16 and Comparative Examples 12-15, it can be seen that, relative to Example 1, the flocculation effect parameters of Examples 13-16 are decreased and the flocculation time is increased, while the flocculation effect parameters of Comparative Examples 12-15 are greatly decreased and the flocculation time is greatly increased. This indicates that the components of the flocculant have a better flocculation effect under the ratio of Example 1.
[0074] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A flocculant, characterized in that: The invention comprises the following raw materials in parts by weight: 16-20 parts of chitin, 4-6 parts of Aspergillus fermentation broth, 2-3 parts of PLA-g-CS, 10-12 parts of epoxy quaternary ammonium salt and 8-12 parts of calcium salt. The Aspergillus fermentation broth contains Aspergillus niger and Aspergillus nidulans. The PLA-g-CS is prepared by grafting chitosan with carboxyl-terminated polylactic acid.
2. The flocculant according to claim 1, characterized in that: The Aspergillus fermentation broth is a mixture of Aspergillus niger fermentation broth and Aspergillus nidulans fermentation broth, and the mass ratio of the Aspergillus niger fermentation broth to the Aspergillus nidulans fermentation broth is (3-5):
1.
3. The flocculant according to claim 1, characterized in that: The preparation method of the PLA-g-CS comprises the following steps: Preparation of carboxyl-terminated polylactic acid: weigh lactide, water, and zinc lactate, mix them evenly, heat them under nitrogen protection to melt the reactants, and obtain carboxyl-terminated polylactic acid; Preparation of PLA-g-CS: dissolving the carboxyl-terminated polylactic acid in dimethyl sulfoxide, adding 1-ethyl-3-dimethylaminopropylcarbodiimide hydrochloride and N-hydroxysuccinimide, stirring at a constant temperature, adding chitosan solution to react, dialyzing to remove impurities, filtering to remove precipitates, and freeze-drying to obtain PLA-g-CS.
4. The flocculant according to claim 3, characterized in that: The mass ratio of the carboxyl-terminated polylactic acid to the chitosan in the chitosan solution is 10:(0.4-0.8).
5. The flocculant according to claim 1, characterized in that: The epoxy quaternary ammonium salt is a mixture of 2,3-epoxypropyl dodecyl dimethyl ammonium chloride and epoxypropyl trimethyl ammonium chloride.
6. The flocculant according to claim 5, characterized in that: The mass ratio of the 2,3-epoxypropyldodecyldimethylammonium chloride to the epoxypropyltrimethylammonium chloride is (1-3):
1.
7. A method for preparing a flocculant, for preparing the flocculant according to any one of claims 1 to 6, characterized in that: Firstly, chitosan, Aspergillus fermentation broth and PLA-g-CS are added into a solvent and stirred sufficiently, then epoxy quaternary ammonium salt and calcium salt are added, and then stirred under UVA environment to finally obtain a flocculant.
8. The method for preparing a flocculant according to claim 7, characterized in that: When stirred under UVA ultraviolet environment, the reaction temperature is 35-40°C and the reaction time is 8-10h.
9. The method for preparing a flocculant according to claim 7, characterized in that: When stirred under UVA ultraviolet environment, the ultraviolet wavelength is 400-405nm and the pH value is 5-7.
10. A sludge dehydration and solidification treatment process, characterized in that: The following steps are involved: Extraction: The sludge slurry is extracted into the sludge pool and then mixed and stirred evenly; Sedimentation: adding the flocculant according to any one of claims 1 to 9 to the sludge slurry, followed by stirring, mixing and sedimentation to obtain stratified sludge floccules and supernatant; Dehydration: Transfer the mud flocs to the geotextile for dehydration and filtration to obtain the solidified mud cake and take it out.
Citation Information
Patent Citations
Method for preparing chitin size modified by biological enzyme method
CN101736583A
Grafted copolymer preparing method based on chitosan and polylactic acid
CN105001425A
Composite biological digestion agent as well as preparation method and application thereof
CN107541469A
Heavy metal solidification stabilizing agent for polluted bottom mud and preparation method thereof
CN108503158A
Treatment agent for high water content dredged (Deposited bottom) mud and its treatment