Sludge heavy metal resource recycling material and preparation method thereof
By combining modified microcrystalline cellulose and cyclic thiochloropropane, a material that efficiently adsorbs heavy metal ions is formed, which solves the problems of high energy consumption, high cost and low efficiency of heavy metal sludge treatment in the prior art, and achieves high efficiency and environmental protection heavy metal resource recycling.
Patent Information
- Application Number
- CN202411078741.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The prior art has problems such as high energy consumption, high cost, unstable treatment effect and secondary pollution in heavy metal sludge treatment, and the biological treatment method is low in efficiency, making it difficult to effectively recover heavy metal resources.
Microcrystalline cellulose is used as the matrix material, and the active groups of S and N elements are added by modification, and cyclic thiochloropropane is combined as a crosslinking agent to form a complex three-dimensional network structure, which enhances the adsorption performance of heavy metal ions, and through The polymerization of dimethylamine and dissilbutylamine improves the stability and reusability of the material.
It has achieved efficient adsorption and recycling of heavy metal ions, reduced industrial costs, improved the stability and reusability of materials, and was able to be recycled multiple times, significantly improving the efficiency and environmental protection of heavy metal resource recycling.
Smart Images

Figure CN118908512A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heavy metal recovery, and specifically refers to a sludge heavy metal resource recovery material and a preparation method thereof. Background Art
[0002] Industrial sludge comes from a wide range of sources, including papermaking sludge, electroplating sludge, textile printing and dyeing, leather making, ore smelting and metallurgy, etc., and its composition is relatively complex. Papermaking sludge is mainly composed of inorganic components, including lignin, chlorine-containing wastewater and sulfur-containing wastewater; the components in electroplating sludge are usually related to the electroplating process, which contains a large amount of heavy metals, such as cadmium, chromium, nickel, copper, manganese, mercury, etc., which exist in the form of soluble heavy metal salts; the leather industry mainly includes a large number of chemical reagents. For example, the use of chrome tanning agents causes a large amount of trivalent chromium salt residues; in the ore smelting and metallurgical industry, the sludge produced is mainly metal ore waste, such as metal oxides such as iron oxides, aluminum oxides, zinc oxides, and heavy metals such as lead, cadmium, nickel, copper, etc. produced during the smelting process, which remain in the sludge in the form of soluble salts. In the existing technology, the main treatment methods for heavy metal sludge include: landfill fixation, heavy metal ions are easy to migrate, usually posing a great threat to the soil environment and groundwater environment; through incineration, pyrolysis and melting heat treatment methods, heavy metals can be concentrated in ash, which is conducive to further resource utilization, but the treatment process consumes a lot of energy, and it is also necessary to match the flue gas purification device, resulting in increased costs, and it is also easy to cause secondary pollution; precipitation treatment by chemical reagents, so that the heavy metals form insoluble precipitates for separation, but the cost of the reagents is high, the treated chemical sludge still needs further treatment, the treatment effect is unstable, and the reaction conditions have a great impact; biological treatment is the most environmentally friendly method, but the treatment cycle is too long and the efficiency is relatively low. Summary of the invention
[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a sludge heavy metal resource recovery material and a preparation method thereof. The present invention uses microcrystalline cellulose as a matrix material, which is mainly a straight-chain polysaccharide substance bonded by β-1,4-glucosidic bonds. It is degradable, green and pollution-free. By modifying the microcrystalline cellulose and increasing the active groups of the S element and the N element, the binding capacity for heavy metal ions is improved, thereby enhancing the adsorption performance.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0005] The present invention also provides a method for preparing sludge heavy metal resource recovery material, which specifically comprises the following steps:
[0006] S1. Dissolve thiourea in deionized water, add sulfuric acid solution, add neutral alumina, mix well, add epichlorohydrin, adjust the water bath temperature to 30-35°C, stir at a speed of 150-180rpm for 20-40min, extract the reactant with a mixed solution of n-hexane and chloroform, collect the organic phase, remove water, and distill under reduced pressure to obtain epichlorohydrin;
[0007] Preferably, in step S1, the mass concentration of thiourea in deionized water is 0.3-0.4 g / mL;
[0008] Preferably, in step S1, the mass fraction of the sulfuric acid solution is 5%, and the added volume of the sulfuric acid solution is 30%-35% of the volume of the thiourea solution; the added amount of the neutral alumina in the thiourea solution is 10-20 g / L;
[0009] Preferably, in step S1, the mass volume ratio of thiourea to epichlorohydrin g / mL is 0.90-0.98 g / mL;
[0010] S2, placing microcrystalline cellulose in deionized water, stirring until completely dispersed, adding sodium hydroxide solution, performing ultrasonic treatment at a power of 400 W for 50-60 min, and stirring the solution until it is uniform to obtain a cellulose solution;
[0011] Preferably, in step S2, the mass fraction of the microcrystalline cellulose in deionized water is 5%-8%;
[0012] Preferably, in step S2, the mass fraction of sodium hydroxide in the sodium hydroxide solution is 10%-20%, and the added volume of the sodium hydroxide solution is 25%-50% of the volume of the microcrystalline cellulose solution;
[0013] S3, dissolving dimethylamine and di-sec-butylamine in deionized water, adding to the cellulose solution prepared in step S2, stirring and mixing evenly, adding epichlorohydrin prepared in step S1, raising the temperature to 65-75°C, stirring and reacting at a speed of 200-220rpm for 2-3h, dialyzing with a dialysis bag with a molecular weight cutoff of 8000-14000 until the solution is neutral, and freeze-drying to obtain sludge heavy metal resource recovery material;
[0014] Preferably, in step S3, the volume ratio between dimethylamine and di-sec-butylamine is 10:1.6-6;
[0015] Preferably, in step S3, the volume ratio between dimethylamine and epichlorohydrin is 0.8-1.2:1;
[0016] The present invention also provides a sludge heavy metal resource recovery material prepared according to the method.
[0017] The beneficial effects achieved by the present invention are as follows:
[0018] The invention provides a sludge heavy metal resource recovery material. The invention uses microcrystalline cellulose as a matrix material and is mainly a linear polysaccharide material bonded by beta-1,4-glucosidic bonds. The material is degradable and green and pollution-free. The microcrystalline cellulose is modified to increase the active groups of S and N elements, thereby improving the binding capacity for pollutants and enhancing the adsorption performance for heavy metals. The invention uses epichlorohydrin as a crosslinking agent to crosslink cellulose molecules. Meanwhile, dimethylamine, di-sec-butylamine and epichlorohydrin are polymerized. An in-situ polymerization reaction occurs while the cellulose undergoes a crosslinking reaction. The polyamine compound and the crosslinked cellulose form a complex three-dimensional network structure, thereby improving the stability of the cellulose and increasing the active sites for the recovery material to adsorb pollutants. Epichlorohydrin can introduce S elements into the recovery material. The sulfur element has an empty electron orbit and can form a coordination effect with heavy metal ions, thereby adsorbing the heavy metal ions. After the heavy metal ions are recovered through a removal treatment, the recovery material has good reusability and can be recycled for multiple times, thereby reducing the recovery industry cost of heavy metal ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Infrared spectra of the sludge heavy metal resource recovery material and microcrystalline cellulose prepared in Example 1 of the present invention;
[0020] Figure 2 This is a SEM image of the sludge heavy metal resource recovery material described in Example 1 of the present invention;
[0021] Figure 3 The adsorption performance results of the recycled materials prepared in Examples 1-3 and Comparative Examples 1-3 on cadmium ions are shown in FIG.
[0022] Figure 4 This is a graph showing the adsorption regeneration performance results of the recycled materials prepared in Examples 1-3 and Comparative Examples 1-3.
[0023] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0025] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0026] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0027] The sources of the materials used in the present invention are as follows:
[0028] Dimethylamine (CasNO: 124-40-3), brand is Macklin, product number is D807422, specification is dimethylamine aqueous solution, 40 wt. % in H2O.
[0029] Microcrystalline cellulose (CasNo: 9004-34-6), brand name Hushi, was purchased from Sinopharm Chemical Reagent Co., Ltd., code number 68005882.
[0030] Example 1
[0031] This embodiment provides a method for preparing a sludge heavy metal resource recovery material, which specifically includes the following steps:
[0032] S1. Accurately weigh 40 g of thiourea and place it in a beaker. Add 100 mL of deionized water and stir until the thiourea is completely dissolved. Prepare a 5% sulfuric acid solution, take 30 mL and add it to the thiourea solution. Add 2 g of neutral alumina, place the solution on a 180 rpm magnetic stirrer and mix evenly, add 36 mL of epichlorohydrin, and under continuous stirring, raise the water bath temperature to 30 ° C. After reacting for 30 minutes, prepare n-hexane and chloroform in a volume ratio of 2:1 to prepare an extractant for extracting the reactants. Extract three times, collect the organic phase, remove excess water in the organic phase with anhydrous sodium sulfate, and remove the organic solvent by vacuum distillation to obtain epichlorohydrin; in this embodiment, 15.38 g of epichlorohydrin is obtained, and its yield is 28.35%; the hydrogen nuclear magnetic resonance spectrum of the product is: 1 HNMR(400MHz, CDCl3)δ3.21(d,2H)2.84-2.69(m,1H),2.41(dd,1H),2.18(d,1H);
[0033] S2. Dry the microcrystalline cellulose in an oven at 35°C to constant weight, accurately weigh 5 g of the dried microcrystalline cellulose and place it in a beaker, add 100 mL of deionized water and stir, completely disperse the microcrystalline cellulose in the deionized water, add 25 mL of a 20% sodium hydroxide solution by mass, mix well, place in an ultrasonic machine and perform ultrasonic treatment at a power of 400 W for 60 min, stir the reaction system continuously during the ultrasonic treatment, and the solution reaches a uniform state to obtain a cellulose solution;
[0034] S3, accurately measure 10 mL of dimethylamine aqueous solution and 1.6 mL of di-sec-butylamine and put them into a flask, stir and mix them evenly, then add the cellulose solution prepared in step S2, continue stirring, take 10 mL of epichlorohydrin prepared in step S1 and dissolve it in 150 mL of 50% ethanol aqueous solution to prepare epichlorohydrin solution, add epichlorohydrin to the reaction system at a rate of 10 mL / min, after the epichlorohydrin solution is added dropwise, seal the reaction system, raise the temperature to 70°C under a nitrogen atmosphere, adjust the stirrer speed to 200 rpm, react for 3 hours, place the reaction system in a 14,000 molecular weight cutoff dialysis bag and dialyze with deionized water until the solution is neutral, and freeze-dry at -50°C and a vacuum degree of <100 Pa to obtain sludge heavy metal resource recovery materials;
[0035] The infrared spectrum images of the sludge heavy metal resource recovery material and microcrystalline fiber were compared. Figure 1 The infrared spectra of the sludge heavy metal resource recovery material and microcrystalline cellulose prepared in this embodiment are as follows: Figure 1 Image 1 is the infrared spectrum image of microcrystalline cellulose, and Image 2 is the sludge heavy metal resource recovery material prepared in this embodiment, at 3500-3300cm -1 There are obvious characteristic peaks at 1650-1620cm -1 The bending vibration peak of NH appears at 1200-1170cm -1 The CS characteristic peak appears at , indicating that epichlorohydrin participates in the cross-linking reaction between cellulose and polyamine compounds;
[0036] This embodiment also provides a sludge heavy metal resource recovery material prepared according to the above method.
[0037] Figure 2 This is the SEM image of the sludge heavy metal resource recovery material described in this embodiment. As shown in the figure, the sample surface is first fractured with liquid nitrogen, and then the sample surface is sprayed with gold after being thoroughly dried. Finally, the sample surface morphology is observed using a JSM-6510 scanning electron microscope. The recovered material has a complex multi-layer network structure.
[0038] Example 2
[0039] This embodiment provides a method for preparing a sludge heavy metal resource recovery material, which specifically includes the following steps:
[0040] S1. Accurately weigh 30 g of thiourea and place it in a beaker. Add 100 mL of deionized water and stir until the thiourea is completely dissolved. Prepare a 5% sulfuric acid solution, take 35 mL and add it to the thiourea solution. Add 1 g of neutral alumina, place the solution on a 180 rpm magnetic stirrer and mix evenly, add 28.52 mL of epichlorohydrin, and under continuous stirring, raise the water bath temperature to 30 ° C. After reacting for 40 minutes, prepare n-hexane and chloroform in a volume ratio of 2:1 to prepare an extractant for extracting the reactants. After three extractions, collect the organic phase, remove excess water in the organic phase with anhydrous sodium sulfate, and remove the organic solvent by vacuum distillation to obtain epichlorohydrin; in this embodiment, 10.23 g of epichlorohydrin is obtained, and its yield is 25.96%;
[0041] S2. Dry the microcrystalline cellulose in an oven at 35°C to constant weight, accurately weigh 8 g of the dried microcrystalline cellulose and place it in a beaker, add 100 mL of deionized water and stir, completely disperse the microcrystalline cellulose in the deionized water, add 50 mL of a 10% sodium hydroxide solution by mass, mix well, place in an ultrasonic machine and perform ultrasonic treatment at a power of 400 W for 60 min, stir the reaction system continuously during the ultrasonic treatment, and the solution reaches a uniform state to obtain a cellulose solution;
[0042] S3, accurately measure 10mL of dimethylamine aqueous solution and 6mL of di-sec-butylamine into a flask, stir and mix evenly, add the cellulose solution prepared in step S2, continue stirring, take 8mL of epichlorohydrin prepared in step S1 and dissolve it in 150mL of 50% ethanol aqueous solution to prepare epichlorohydrin solution, add epichlorohydrin into the reaction system at a rate of 10mL / min, after the epichlorohydrin solution is added dropwise, seal the reaction system, raise the temperature to 75°C under a nitrogen atmosphere, adjust the stirrer speed to 200rpm, react for 3h, place the reaction system in a 12000 molecular weight cutoff dialysis bag and dialyze with deionized water until the solution is neutral, place it at -50°C and a vacuum degree of <100pa, and freeze-dry it to obtain sludge heavy metal resource recovery material;
[0043] This embodiment also provides a sludge heavy metal resource recovery material prepared according to the above method.
[0044] Example 3
[0045] This embodiment provides a method for preparing a sludge heavy metal resource recovery material, which specifically includes the following steps:
[0046] S1. Accurately weigh 35 g of thiourea and place it in a beaker. Add 100 mL of deionized water and stir until the thiourea is completely dissolved. Prepare a 5% sulfuric acid solution, take 30 mL and add it to the thiourea solution. Add 1.5 g of neutral alumina, place the solution on a 150 rpm magnetic stirrer and mix evenly, add 34.3 mL of epichlorohydrin, and under continuous stirring, raise the water bath temperature to 35 ° C. After reacting for 20 minutes, prepare n-hexane and chloroform in a volume ratio of 2:1 to prepare an extractant for extracting the reactants. After three extractions, collect the organic phase, remove excess water in the organic phase with anhydrous sodium sulfate, and remove the organic solvent by vacuum distillation to obtain epichlorohydrin; in this embodiment, 12.74 g of epichlorohydrin is obtained, and its yield is 26.84%;
[0047] S2. Dry the microcrystalline cellulose in an oven at 35°C to constant weight, accurately weigh 6.5 g of the dried microcrystalline cellulose and place it in a beaker, add 100 mL of deionized water and stir, completely disperse the microcrystalline cellulose in the deionized water, add 35 mL of a 20% sodium hydroxide solution by mass, mix well, place in an ultrasonic machine and perform ultrasonic treatment at a power of 400 W for 50 min, stir the reaction system continuously during the ultrasonic treatment, and the solution reaches a uniform state to obtain a cellulose solution;
[0048] S3, accurately measure 10mL of dimethylamine aqueous solution and 3.6mL of di-sec-butylamine into a flask, stir and mix evenly, add 100mL of the cellulose solution prepared in step S2, continue stirring, take 12mL of epichlorohydrin prepared in step S1 and dissolve it in 150mL of 50% ethanol aqueous solution to prepare epichlorohydrin solution, add epichlorohydrin into the reaction system at a rate of 10mL / min, after the epichlorohydrin solution is added dropwise, seal the reaction system, raise the temperature to 65°C under a nitrogen atmosphere, adjust the stirrer speed to 220rpm, react for 2h, place the reaction system in a 8000 molecular weight cutoff dialysis bag and dialyze with deionized water until the solution is neutral, place it at -50°C and a vacuum degree of <100pa, and freeze-dry it to obtain sludge heavy metal resource recovery material;
[0049] This embodiment also provides a sludge heavy metal resource recovery material prepared according to the above method.
[0050] Comparative Example 1
[0051] This comparative example provides a heavy metal recovery material and a preparation method thereof, which differs from Example 1 only in that the preparation method of the heavy metal recovery material does not include step S1, and step S3 does not include epichlorohydrin, and the remaining components, component contents and preparation methods are the same as those in Example 1.
[0052] Comparative Example 2
[0053] This comparative example provides a heavy metal recovery material and a preparation method thereof, which differs from Example 1 only in that the preparation method of the heavy metal recovery material does not include step S3, and only the cellulose solution is cross-linked with epichlorohydrin, and the remaining components, component contents and preparation methods are the same as those in Example 1.
[0054] Comparative Example 3
[0055] This comparative example provides a heavy metal recovery material and a preparation method thereof, which differs from Example 1 only in that, in step S3 of the preparation method of the heavy metal recovery material, dimethylamine and di-sec-butylamine are dissolved in deionized water, epichlorohydrin prepared in step S1 is added, and after polymerization reaction, the cellulose solution prepared in step S2 is added, and after mixing, the heavy metal recovery material is obtained by drying, and the remaining components, component contents and preparation method are the same as those in Example 1.
[0056] Experimental Example 1
[0057] In this experimental example, an adsorption test was performed on the heavy metal recovery materials prepared in Examples 1-3 and Comparative Examples 1-3. A 50 mg / L cadmium ion solution was prepared with cadmium chloride, 50 mL was measured and placed in a conical flask, the pH was adjusted to 7, 50 mg of the heavy metal recovery materials prepared in Examples 1-3 and Comparative Examples 1-3 were added, placed at room temperature, and oscillated at 200 rpm. Samples were taken at 5 min, 10 min, 20 min, 30 min, 45 min, 60 min, 75 min, 90 min, 120 min, 150 min, 180 min, and 240 min, and the cadmium ion concentration in the supernatant was determined by ICP-OES after passing through an aqueous phase filter membrane.
[0058] Figure 3The adsorption performance results of the recycled materials prepared in Examples 1-3 and Comparative Examples 1-3 for cadmium ions are shown in the figure. As shown in the figure, the adsorption of tetracycline by the recycled materials prepared in Examples 1-3 reaches equilibrium at about 90 minutes, and the adsorption capacity after equilibrium reaches 71.3-72.5 mg / g. The recycled material prepared in Comparative Example 2 reaches equilibrium at about 150 minutes, and the adsorption capacity after equilibrium is 36.5 mg / g. The recycled material prepared in Comparative Example 1 reaches equilibrium at about 120 minutes, and the adsorption capacity after equilibrium is 48.3 mg / g. The recycled material prepared in Comparative Example 3 reaches equilibrium at about 1 It takes about 80 minutes to reach equilibrium, and the adsorption capacity after equilibrium is 54.8 mg / g; the adsorption capacity of Comparative Examples 1 and 3 after equilibrium shows a decrease in adsorption capacity, indicating that the prepared heavy metal recovery material has desorption of cadmium ions, indicating that the adsorption performance of the heavy metal recovery material is unstable. The heavy metal recovery material prepared by the present invention has high adsorption performance for cadmium ions and can achieve a higher adsorption capacity. At the same time, the adsorption performance is stable. The recovery material prepared in the comparative example has significantly fewer adsorption sites, so the adsorption capacity is low, and desorption still exists.
[0059] Experimental Example 2
[0060] In this experimental example, the recycled materials prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to an adsorption regeneration test on cadmium ions. 50 mg of the recycled materials prepared in Examples 1-3 and Comparative Examples 1-3 were taken as test samples. The pH was adjusted to 7 in a 50 mg / L cadmium ion solution. The solution was shaken at 200 rpm at room temperature for 300 min. The adsorption capacity of the test sample was measured. The test sample was filtered and separated. After soaking in a 0.1 mol / L hydrochloric acid solution for 3 h, it was washed and dried with deionized water. The adsorption test was performed again. The adsorption-desorption cycle was performed. After 5 cycles, the adsorption capacity of the fifth test sample was measured and compared with the initial adsorption capacity.
[0061] Figure 4The adsorption regeneration performance result diagram of the recycled materials prepared in Examples 1-3 and Comparative Examples 1-3 is shown in the figure. As shown in the figure, after 5 regeneration treatments, the adsorption capacities of the recycled materials prepared in Examples 1-3 reach 60.3 mg / g, 59.2 mg / g, and 58.740 mg / g or more, respectively. After 5 regeneration treatments, the adsorption capacity of the recycled material prepared in Comparative Example 1 decreases to 15.5 mg / g. After 5 regeneration treatments, the adsorption capacity of the recycled material prepared in Comparative Example 2 decreases to 2.4 mg / g. After 5 regeneration treatments, the adsorption capacity of the recycled material prepared in Comparative Example 1 decreases to 25.1 mg / g; it shows that the recycled material prepared in the present invention has good stability and can be recycled. The recycled material prepared in Comparative Example 1 modifies cellulose with dimethylamine and di-sec-butylamine through intermolecular forces, lacks the crosslinking effect of the sulfur-containing crosslinking agent, and reduces the interaction between the cellulose material and the polyamine, resulting in the recycling material having a low initial adsorption rate of heavy metal ions. The rate is slow, and at the same time, the adsorption active sites are significantly reduced, resulting in a decrease in adsorption capacity. After multiple cycles, the structure of the recycled material is destroyed, the active sites are passivated, and the adsorption of heavy metal ions by the active sites cannot be desorbed, further resulting in a decrease in the utilization of the recycled material; the recycled material prepared in Comparative Example 2 is actually cellulose cross-linked with epichlorohydrin. After the cellulose is cross-linked, groups containing S elements are introduced into the cellulose molecules, increasing the adsorption active sites, and the adsorption rate is the slowest. After cross-linking, the cellulose molecules are close, and the contact between the active sites and the heavy metal ions is not sufficient. After the adsorption treatment, the heavy metal ions are difficult to desorb from the recycled material, resulting in a significant decrease in the reuse performance. In the recycled material prepared in Comparative Example 3, dimethylamine, di-sec-butylamine and epichlorohydrin are first polymerized to form a polyamine compound, which is then physically blended with cellulose. A complex network structure is not formed between the polyamine compound and the cellulose, resulting in a decrease in adsorption performance, and also resulting in a decrease in the stability of the recycled material.
[0062] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
[0063] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing sludge heavy metal resource recovery materials, characterized in that: The specific steps include: S1. Dissolve thiourea in deionized water, add sulfuric acid solution, add neutral alumina, mix well, add epichlorohydrin, adjust the water bath temperature to 30-35°C, stir at a speed of 150-180rpm for 20-40min, extract the reactant with a mixed solution of n-hexane and chloroform, remove water, and distill under reduced pressure to obtain epichlorohydrin; S2, placing microcrystalline cellulose in deionized water, stirring until completely dispersed, adding sodium hydroxide solution, performing ultrasonic treatment at a power of 400 W for 50-60 min, and stirring the solution until it is uniform to obtain a cellulose solution; S3. Dissolve dimethylamine and di-sec-butylamine in deionized water, add to the cellulose solution prepared in step S2, stir and mix evenly, add epichlorohydrin prepared in step S1, raise the temperature to 65-75° C., stir and react at a speed of 200-220 rpm for 2-3 hours, dialyze with a dialysis bag with a molecular weight cutoff of 8000-14000 until the solution is neutral, and freeze-dry to obtain sludge heavy metal resource recovery material.
2. The method for preparing a sludge heavy metal resource recovery material according to claim 1, characterized in that: In step S1, the mass concentration of thiourea in deionized water is 0.3-0.4 g / mL.
3. The method for preparing a sludge heavy metal resource recovery material according to claim 2, characterized in that: In step S1, the mass volume ratio of thiourea to epichlorohydrin g / mL is 0.90-0.98 g / mL.
4. The method for preparing a sludge heavy metal resource recovery material according to claim 3, characterized in that: In step S1, the mass fraction of the sulfuric acid solution is 5%, and the added volume of the sulfuric acid solution is 30%-35% of the volume of the thiourea solution.
5. The method for preparing a sludge heavy metal resource recovery material according to claim 4, characterized in that: In step S1, the amount of neutral alumina added to the thiourea solution is 10-20 g / L.
6. The method for preparing a sludge heavy metal resource recovery material according to claim 5, characterized in that: In step S2, the mass fraction of the microcrystalline cellulose in deionized water is 5%-8%.
7. The method for preparing a sludge heavy metal resource recovery material according to claim 6, characterized in that: In step S2, the mass fraction of sodium hydroxide in the sodium hydroxide solution is 10%-20%, and the added volume of the sodium hydroxide solution is 25%-50% of the volume of the microcrystalline cellulose solution.
8. The method for preparing a sludge heavy metal resource recovery material according to claim 7, characterized in that: In step S3, the volume ratio of dimethylamine to di-sec-butylamine is 10:1.6-6.
9. The method for preparing a sludge heavy metal resource recovery material according to claim 8, characterized in that: In step S3, the volume ratio between dimethylamine and epichlorohydrin is 0.8-1.2:
1.
10. A sludge heavy metal resource recovery material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Moisture-absorbing agent, flocculation aid, and desiccant for general waste and its manufacturing process.
BR102020001136A2
Manufacturing of paper with biocides
CA2839129A1
Resin barrier control agent added with modified nano microcrystalline cellulose and preparation method of resin barrier control agent
CN104452444A
Preparation method and application of functional biomass charcoal-based adsorbent
CN113083254A
Preparation method of supported chelating resin-based water treatment adsorption material
CN115487787A