Method for preparing aromatic compound and co-producing heavy metal adsorption material by carrying out in-situ catalytic pyrolysis on waste thermosetting phenolic resin by using red mud

Through the in-situ catalytic pyrolysis technology of red mud, aromatic compounds are produced and heavy metal adsorbent materials are solved, and the recycling and pollution control problems of waste thermosetting phenolic resins and red mud are achieved, achieving efficient recycling and coordinated emission reduction of pollutants.

CN118908519AActive Publication Date: 2024-11-08SHANDONG UNIV OF TECH

Patent Information

Application Number
CN202410960435.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently recycle and utilize waste thermosetting phenolic resins, and the environmental pollution and resource waste of red mud have not been effectively solved.

Method used

Through the in-situ catalytic pyrolysis technology of red mud, citric acid is used to soak the red mud and perform ammonia water regulation, filtration, drying and high-temperature roasting, activated red mud catalyst is prepared, and mixed with waste thermosetting phenolic resin for in-situ catalytic pyrolysis reaction. Prepare heavy metal adsorbent materials for co-producing aromatic compounds for use in the treatment of sewage in electroplating industry.

Benefits of technology

It has achieved efficient recycling of waste thermosetting phenolic resins and industrial catalytic application of red mud, reduced environmental pollution, improved heavy metal adsorption efficiency, and promoted the coordinated pollution reduction and carbon reduction control of multi-source pollutants.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of multi-source pollutant synergistic prevention and control, and particularly relates to a method for preparing aromatic compounds and co-producing a heavy metal adsorption material through red mud in-situ catalytic pyrolysis of waste thermosetting phenolic resin. According to the method for preparing the aromatic compound and co-producing the heavy metal adsorption material through in-situ catalytic pyrolysis of the waste thermosetting phenolic resin by using the red mud, firstly, the red mud is subjected to modification treatment, and a low-cost activated red mud catalyst material is obtained; then putting a mixed raw material of the waste thermosetting phenolic resin and the activated red mud catalyst material into a catalytic upgrading reactor to realize catalytic degradation and recycling of the waste thermosetting phenolic resin and co-produce a heavy metal adsorption material rich in zero-valent iron; and finally, applying the prepared adsorption material to a treatment link of electroplating industrial sewage containing heavy metals. The whole technical method is simple in process operation and high in generalizability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coordinated prevention and control of multi-source pollutants, and specifically relates to a method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin through red mud. Background Art

[0002] Phenolic resin is mainly a dimer compound generated by the polycondensation reaction of phenol and formaldehyde. It is divided into two categories: thermoplastic phenolic resin and thermosetting phenolic resin. It is widely used in the automobile manufacturing industry, construction engineering industry, household appliance industry, machinery manufacturing industry and aerospace field. In recent years, the output and demand of phenolic resin in my country have steadily increased, and supply and demand have maintained a tight balance, accompanied by the generation of a large amount of waste phenolic resin. It is worth noting that thermosetting phenolic resin no longer softens after being hardened by heat, and its complex chemical properties and thermal stability are not conducive to recycling. Therefore, how to efficiently recycle waste thermosetting phenolic resin is of great significance for resource reuse and reducing environmental pollution.

[0003] The recycling technologies of waste thermosetting phenolic resins mainly include physical recycling, chemical recycling, thermal energy recycling and thermal cracking recycling. Among them, thermal cracking recovery technology has the characteristics of high reaction conversion recovery efficiency and high carbon effective conversion rate. It is one of the feasible technologies for efficient recovery of thermosetting phenolic resins, but there are still problems such as difficult regulation of the pyrolysis process and poor product quality. At present, in-situ catalytic pyrolysis technology can enhance the heat and mass transfer process, reduce the reaction activation energy, adjust the pyrolysis gas reconstruction path and the carbon-based material skeleton by introducing catalysts, so as to achieve the preparation of high value-added products. In addition, by improving the carbon utilization level and reducing energy input, it directly or indirectly promotes the reduction of carbon emissions from the pyrolysis system. Therefore, how to develop a new low-carbon pyrolysis technology suitable for thermosetting phenolic resins is the key to achieving its efficient recovery.

[0004] Red mud is an aluminum smelting waste produced by the alumina industry. Its large-scale accumulation causes serious environmental pollution and waste of resources. At present, red mud can be modified by acid treatment, alkaline activation and other means to improve its pore structure and enhance catalytic active sites, which is expected to show unique advantages in the catalytic pyrolysis conversion of waste thermosetting phenolic resin. Therefore, how to achieve precise control of the process of in-situ catalytic pyrolysis of waste thermosetting phenolic resin to produce aromatic compounds and co-produce heavy metal adsorption materials is of great significance to the development of a technology system for the coordinated reduction of pollution and carbon emissions from multiple sources of pollutants such as waste thermosetting phenolic resin, red mud, and heavy metals. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin by red mud. The method realizes the efficient recovery of waste thermosetting phenolic resin, the industrial catalytic application of red mud, and the treatment of heavy metal-containing electroplating industrial wastewater, providing a technical reference for the coordinated reduction of pollution and carbon emissions from multiple sources of pollutants.

[0006] The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin by red mud of the present invention comprises the following steps:

[0007] (1) firstly, leaching red mud with citric acid, adjusting it to neutral with ammonia water, then filtering it, washing it with ethanol and deionized water, and then drying it, and finally calcining the obtained solids at high temperature to obtain an activated red mud catalyst material;

[0008] (2) mixing the activated red mud catalyst material obtained in step (1) with waste thermosetting phenolic resin in a certain proportion and placing the mixture in a catalytic upgrading reactor for in-situ catalytic pyrolysis reaction to produce an aromatic compound co-production adsorption material;

[0009] (3) Adding the adsorption material prepared in step (2) to the electroplating industrial wastewater containing heavy metals to carry out an adsorption reaction, thereby achieving coordinated pollution reduction and carbon reduction of multiple sources of pollutants.

[0010] in:

[0011] The red mud raw material used in step (1) is solid waste residue produced by the Bayer process for preparing alumina, and its specific chemical composition, in terms of mass percentage, is as follows: Na2O 13.01-13.92%, MgO 0.21-0.35%, Al2O3 22.58-23.20%, SiO2 18.75-20.12%, Fe2O3 22.50-23.24%, K2O 0.38-0.47%, TiO2 1.85-2.23%, CaO 8.79-9.52%, ZrO2 0.06-0.09%, and loss on ignition 8.87-9.86%.

[0012] In step (1), the concentration of citric acid is 1-3 mol / L, and the mass fraction of ammonia water is 36%.

[0013] In step (1), the mass volume ratio of red mud to citric acid is 5:20-60, in g / mL.

[0014] In step (1), the acid leaching temperature is 80-83° C., and the acid leaching time is 40-45 min.

[0015] In step (1), the drying temperature is 100-105° C. and the drying time is 24 h.

[0016] In step (1), the high temperature calcination is carried out by heating the temperature from room temperature to 600-800° C. at a heating rate of 5° C. / min for 2-4 hours.

[0017] The activation treatment of red mud in step (1) can effectively remove the Na and Ca elements in the red mud, reduce the strong alkalinity of the red mud, promote structural reorganization, and at the same time make the red mud have a higher specific surface area, developed pore characteristics, abundant acid sites and catalytically active metal oxide components. These enhanced structural characteristics can play a role in the catalytic reforming of thermosetting phenolic resin pyrolysis gas.

[0018] In step (2), the mass ratio of the waste thermosetting phenolic resin to the activated red mud catalyst material is 0.5-2:1.

[0019] The reaction atmosphere during the in-situ catalytic pyrolysis reaction in step (2) is one of nitrogen or argon, and the gas flow rate is 100 mL / min; the temperature is increased to the in-situ catalytic pyrolysis reaction temperature at a heating rate of 10°C / min, the in-situ catalytic pyrolysis reaction temperature is 450-650°C, and the in-situ catalytic pyrolysis reaction time is 20-40 min.

[0020] The waste thermosetting phenolic resin in step (2) is one of waste phenol-type phenolic resin, waste bisphenol A phenolic resin or waste biphenyl aralkyl phenolic resin.

[0021] In step (2), the liquid product in the in-situ catalytic pyrolysis product is an aromatic compound, and the solid product in the in-situ catalytic pyrolysis product is an adsorption material.

[0022] In step (3), the mass ratio of the adsorbent to the volume of the electroplating industrial wastewater containing heavy metals is 2.3-3.0:1, expressed in mg / mL, the adsorption reaction time is 12-24h, and the adsorption reaction temperature is 25-35°C.

[0023] The heavy metal-containing electroplating industrial wastewater in step (3) has a zinc ion content of ≤50 mg / L, a copper ion content of ≤30 mg / L, and a pH value of 3.0-3.5.

[0024] The multi-source pollutants in step (3) refer to waste thermosetting phenolic resin, red mud, and electroplating industrial wastewater containing heavy metals.

[0025] The method of the present invention for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin with red mud, on the one hand, the modified red mud rich in active metal oxides (Fe2O3, Al2O3 and TiO2, etc.) and developed pore structure can promote the deoxygenation and quality improvement of the pyrolysis gas of the waste thermosetting phenolic resin, and increase the proportion of aromatic compounds in the liquid product. At the same time, the waste thermosetting phenolic resin can be used as a carbon source to reduce the valence state of the iron oxide compounds rich in the modified red mud, and synthesize a high-efficiency zero-valent iron adsorption material for the treatment of electroplating industrial wastewater containing heavy metals, thereby improving the application value of the catalytic pyrolysis products.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The method of the present invention for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin with red mud comprises the following steps: firstly, red mud is modified to obtain a low-cost activated red mud catalyst material; then, the mixed raw material of the waste thermosetting phenolic resin and the activated red mud catalyst material is placed in a catalytic upgrading reactor to achieve catalytic degradation and reuse of the waste thermosetting phenolic resin and co-production of heavy metal adsorption materials rich in zero-valent iron; finally, the prepared adsorption material is used in the treatment of heavy metal-containing electroplating industrial wastewater; the entire technical method process is simple to operate and has strong scalability.

[0028] (2) The method of the present invention for producing aromatic compounds and heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin with red mud utilizes low-cost activated red mud catalyst materials to improve the quality of waste thermosetting phenolic resin pyrolysis gas, thereby realizing the directional preparation of high-value aromatic compounds such as phenol and aromatics; at the same time, the carbon thermal reduction process during the catalytic pyrolysis process modulates the valence distribution of the activated red mud iron element, and the activated red mud acts as an "in-situ activator" to promote the development of the pore structure of the carbon material, thereby realizing the directional preparation of carbon-iron composite adsorption materials. The new low-carbon pyrolysis technology based on the directional preparation of high-value-added aromatic compounds and carbon-iron composite adsorption materials directly or indirectly promotes the reduction of carbon emissions from the pyrolysis system by improving the carbon utilization level and reducing the reaction activation energy.

[0029] (3) The method of the present invention for producing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin with red mud, the carbon-iron composite adsorption material shows excellent performance in the field of electroplating industrial wastewater treatment containing heavy metals, and realizes the coordinated pollution reduction and carbon reduction of waste thermosetting phenolic resin-red mud-electroplating industrial wastewater containing heavy metals. It has certain promotion and utilization value from the perspective of coordinated prevention and control of multi-source pollutants and sustainable development. DETAILED DESCRIPTION

[0030] The present invention is further described below with reference to the embodiments.

[0031] Example 1

[0032] The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin by red mud described in Example 1 is composed of the following steps:

[0033] (1) 5 g of red mud raw material was mixed with 30 mL of citric acid solution (concentration of 2 mol / L), and digested by acid leaching at 80 ° C for 45 min. Then, 36% ammonia water was added dropwise under uniform stirring to adjust to neutrality. Then, the mixture was washed with ethanol and deionized water for 3 times and dried in an air drying oven at 105 ° C for 24 h. Finally, the obtained solid was calcined in a muffle furnace at a heating rate of 5 ° C / min from room temperature to 600 ° C for 4 h to obtain an activated red mud catalyst material.

[0034] in:

[0035] The red mud raw material used in Example 1 comes from the solid waste residue produced by the Bayer process for preparing alumina. The specific chemical composition, by mass percentage, is as follows: Na2O13.47%, MgO 0.28%, Al2O3 22.85%, SiO2 19.44%, Fe2O322.87%, K2O 0.43%, TiO2 2.04%, CaO 9.16%, ZrO2 0.08%, and loss on ignition 9.38%.

[0036] The activated red mud catalyst material has the following specific chemical composition, calculated by mass percentage: Na2O 0.18%, MgO 0.25%, Al2O3 22.24%, SiO2 25.89%, Fe2O3 39.40%, K2O 0.34%, TiO2 2.81%, CaO 1.87%, ZrO2 0.16%, and loss on ignition 6.86%.

[0037] (2) The activated red mud catalyst material and the waste phenol-type phenolic resin were mixed in a mass ratio of 1:1 and placed in a catalytic upgrading reactor for catalytic pyrolysis reaction to produce aromatic compound co-production adsorption material. The reaction atmosphere was nitrogen, the nitrogen flow rate was 100 mL / min, the reaction temperature was 550°C, the heating rate was 10°C / min, and the pyrolysis time was 30 min. In the liquid products of the in-situ catalytic pyrolysis products, the relative content of aromatic hydrocarbons was 33.23%, the relative content of phenolic compounds was 59.56%, and the selectivity of aromatic compounds could reach 92.79%; the solid products of the in-situ catalytic pyrolysis were used as heavy metal adsorption materials.

[0038] (3) The zinc ion content of the electroplating industrial wastewater containing heavy metals is 25 mg / L, the copper ion content is 20 mg / L, and the pH value is 3.5. 50 mg of the heavy metal adsorption material produced by pyrolysis co-production is placed in 21.5 mL of the electroplating industrial wastewater containing heavy metals, and shaken at 150 r / min in a 35°C air bath constant temperature shaker for 12 hours. Then, the zinc ion concentration and copper ion concentration in the upper suspension are measured by inductively coupled plasma emission spectrometry to calculate the removal efficiency. The zinc ion removal rate is 98.76%, and the copper ion removal rate is 98.13%.

[0039] Example 2

[0040] The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin by red mud described in Example 2 is composed of the following steps:

[0041] (1) 5 g of red mud raw material was mixed with 60 mL of citric acid solution (concentration of 1 mol / L), and digested by acid leaching at 81°C for 43 min. Then, 36% ammonia water was added dropwise under uniform stirring to adjust to neutrality. Then, the mixture was washed with ethanol and deionized water for 3 times and dried in an air drying oven at 100°C for 24 h. Finally, the obtained solid was calcined in a muffle furnace at a heating rate of 5°C / min from room temperature to 700°C for 3 h to obtain an activated red mud catalyst material.

[0042] in:

[0043] The red mud raw material used comes from the solid waste residue produced by the Bayer process for preparing alumina. The specific chemical composition, in terms of mass percentage, is as follows: Na2O 13.01%, MgO 0.35%, Al2O3 22.58%, SiO2 20.12%, Fe2O322.50%, K2O 0.47%, TiO2 2.23%, CaO 8.79%, ZrO2 0.09%, and loss on ignition 9.86%.

[0044] The activated red mud catalyst material has the following specific chemical composition, calculated by mass percentage: Na2O 0.20%, MgO 0.31%, Al2O3 22.17%, SiO2 27.53%, Fe2O3 38.61%, K2O 0.33%, TiO2 3.02%, CaO 1.24%, ZrO2 0.18%, and loss on ignition 6.41%.

[0045] (2) The activated red mud catalyst material and the waste bisphenol A phenolic resin were mixed in a mass ratio of 2:1 and placed in a catalytic upgrading reactor for catalytic pyrolysis reaction to produce aromatic compound co-production adsorption material. The reaction atmosphere was nitrogen, the nitrogen flow rate was 100 mL / min, the reaction temperature was 450°C, the heating rate was 10°C / min, and the pyrolysis time was 40 min. In the liquid products of the in-situ catalytic pyrolysis products, the relative content of aromatic hydrocarbons was 34.27%, the relative content of phenolic compounds was 58.45%, and the selectivity of aromatic compounds could reach 92.72%; the solid products of the in-situ catalytic pyrolysis were used as heavy metal adsorption materials.

[0046] (3) The zinc ion content of the electroplating industrial wastewater containing heavy metals is 35 mg / L, the copper ion content is 25 mg / L, and the pH value is 3.3. 60 mg of the heavy metal adsorption material produced by pyrolysis co-production is placed in 22 mL of the electroplating industrial wastewater containing heavy metals and shaken at 150 r / min in a 25°C air bath constant temperature shaker for 24 hours. Then, the zinc ion concentration and copper ion concentration in the upper suspension are measured by inductively coupled plasma emission spectrometry to calculate the removal efficiency. The zinc ion removal rate is 99.02%, and the copper ion removal rate is 98.89%.

[0047] Example 3

[0048] The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin by red mud described in Example 3 is composed of the following steps:

[0049] (1) 5 g of red mud raw material was mixed with 20 mL of citric acid solution (concentration of 3 mol / L), and digested by acid leaching at 83 °C for 40 min. Then, 36% ammonia water was added dropwise under uniform stirring to adjust to neutrality. Then, the mixture was washed with ethanol and deionized water for 3 times and dried in an air drying oven at 103 °C for 24 h. Finally, the obtained solid was calcined in a muffle furnace at a heating rate of 5 °C / min from room temperature to 800 °C for 2 h to obtain an activated red mud catalyst material.

[0050] in:

[0051] The red mud raw material used comes from the solid waste residue produced by the Bayer process for preparing alumina. The specific chemical composition, in terms of mass percentage, is as follows: Na2O13.92%, MgO 0.21%, Al2O3 23.20%, SiO2 18.75%, Fe2O323.24%, K2O 0.38%, TiO2 1.85%, CaO 9.52%, ZrO2 0.06%, and loss on ignition 8.87%.

[0052] The activated red mud catalyst material has the following specific chemical composition, calculated by mass percentage: Na2O 0.25%, MgO 0.17%, Al2O3 22.68%, SiO2 26.59%, Fe2O3 39.32%, K2O 0.25%, TiO2 2.61%, CaO 1.36%, ZrO2 0.14%, and loss on ignition 6.63%.

[0053] (2) The activated red mud catalyst material and the waste biphenyl aralkyl phenolic resin were mixed in a mass ratio of 1:2 and placed in a catalytic upgrading reactor for catalytic pyrolysis reaction to produce aromatic compound co-production adsorption material. The reaction atmosphere was nitrogen, the nitrogen flow rate was 100 mL / min, the reaction temperature was 650°C, the heating rate was 10°C / min, and the pyrolysis time was 20 min. In the liquid products of the in-situ catalytic pyrolysis products, the relative content of aromatic hydrocarbons was 38.19%, the relative content of phenolic compounds (phenol, methylphenol and dimethylphenol) was 57.20%, and the selectivity of aromatic compounds could reach 95.39%; the solid products of the in-situ catalytic pyrolysis were used as heavy metal adsorption materials.

[0054] (3) The zinc ion content of the heavy metal electroplating industrial wastewater was 45 mg / L, the copper ion content was 30 mg / L, and the pH value was 3.0. 69 mg of the heavy metal adsorption material produced by pyrolysis was placed in 23 mL of the heavy metal electroplating industrial wastewater and shaken at 150 r / min in a 30°C air bath constant temperature shaker for 18 hours. Then, the zinc ion concentration and copper ion concentration in the upper suspension were measured by inductively coupled plasma emission spectrometry to calculate the removal efficiency. The zinc ion removal rate was 99.12%, and the copper ion removal rate was 99.08%.

[0055] Comparative Example 1

[0056] The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin by red mud described in Comparative Example 1 is composed of the following steps:

[0057] (1) 5g of red mud raw material and waste phenol-type phenolic resin were mixed in a mass ratio of 1:1 and placed in a catalytic upgrading reactor for catalytic pyrolysis reaction to produce aromatic compound co-production adsorption material. The reaction atmosphere was nitrogen, the nitrogen flow rate was 100mL / min, the reaction temperature was 550℃, the heating rate was 10℃ / min, and the pyrolysis time was 30min. In the liquid products of the in-situ catalytic pyrolysis products, the relative content of aromatic hydrocarbons was 17.81%, the relative content of phenolic compounds was 71.94%, and the selectivity of aromatic compounds could reach 89.75%; the solid products of the in-situ catalytic pyrolysis were used as heavy metal adsorption materials;

[0058] Among them: the red mud raw material used comes from the solid waste residue produced by the Bayer process for preparing alumina. The specific chemical composition, calculated by mass percentage, is as follows: Na2O13.47%, MgO 0.28%, Al2O3 22.85%, SiO2 19.44%, Fe2O322.87%, K2O 0.43%, TiO2 2.04%, CaO 9.16%, ZrO2 0.08%, and loss on ignition 9.38%.

[0059] (2) The zinc ion content of the electroplating industrial wastewater containing heavy metals is 25 mg / L, the copper ion content is 20 mg / L, and the pH value is 3.5. 50 mg of the heavy metal adsorption material produced by pyrolysis co-production is placed in 21.5 mL of the electroplating industrial wastewater containing heavy metals, and shaken at 150 r / min in a 35°C air bath constant temperature shaker for 12 hours. Then, the zinc ion concentration and copper ion concentration in the upper suspension are measured by inductively coupled plasma emission spectrometry to calculate the removal efficiency. The zinc ion removal rate is 96.45%, and the copper ion removal rate is 96.32%.

[0060] Comparative Example 2

[0061] The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by pyrolyzing waste thermosetting phenolic resin described in Comparative Example 2 is composed of the following steps:

[0062] (1) The waste phenol-type phenolic resin was placed in a catalytic upgrading reactor for catalytic pyrolysis reaction to produce aromatic compound co-production adsorption material. The reaction atmosphere was nitrogen, the nitrogen flow rate was 100 mL / min, the reaction temperature was 550°C, the heating rate was 10°C / min, and the pyrolysis time was 30 min. In the liquid products of the pyrolysis products, the relative content of aromatic hydrocarbons was 4.33%, the relative content of phenolic compounds was 86.53%, and the selectivity of aromatic compounds could reach 90.86%; the phenolic resin charcoal produced by in-situ catalytic pyrolysis was used as a heavy metal adsorption material.

[0063] (2) The zinc ion content of the electroplating industrial wastewater containing heavy metals is 25 mg / L, the copper ion content is 20 mg / L, and the pH value is 3.5. 50 mg of the heavy metal adsorption material produced by pyrolysis co-production is placed in 21.5 mL of the electroplating industrial wastewater containing heavy metals, and shaken at 150 r / min in a 35°C air bath constant temperature shaker for 12 hours. Then, the zinc ion concentration and copper ion concentration in the upper suspension are measured by inductively coupled plasma emission spectrometry to calculate the removal efficiency. The zinc ion removal rate is 95.46%, and the copper ion removal rate is 95.71%.

[0064] In summary, in Comparative Example 1, the red mud is no longer activated, and the red mud raw material and the waste thermosetting phenolic resin are directly pyrolyzed in situ, which is not conducive to the formation of aromatic compounds and reduces the heavy metal removal efficiency. In Comparative Example 2, no activated red mud is added during the pyrolysis of the waste thermosetting phenolic resin, resulting in a significant decrease in the content of aromatic compounds and a decrease in the heavy metal removal efficiency.

Claims

1. A method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud, characterized in that: It consists of the following steps: (1) firstly, leaching red mud with citric acid, adjusting it to neutral with ammonia water, then filtering it, washing it with ethanol and deionized water, and then drying it, and finally calcining the obtained solids at high temperature to obtain an activated red mud catalyst material; (2) mixing the activated red mud catalyst material obtained in step (1) with waste thermosetting phenolic resin in a certain proportion and placing the mixture in a catalytic upgrading reactor for in-situ catalytic pyrolysis reaction to produce an aromatic compound co-production adsorption material; (3) Adding the adsorption material prepared in step (2) to the electroplating industrial wastewater containing heavy metals to carry out an adsorption reaction, thereby achieving coordinated pollution reduction and carbon reduction of multiple sources of pollutants.

2. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: The red mud raw material used in step (1) comes from the solid waste residue produced by the Bayer process for preparing alumina, and its specific chemical composition, measured by mass percentage, is as follows: Na2O 13.01-13.92%, MgO 0.21-0.35%, Al2O3 22.58-23.20%, SiO2 18.75-20.12%, Fe2O3 22.50-23.24%, K2O 0.38-0.47%, TiO2 1.85-2.23%, CaO 8.79-9.52%, ZrO2 0.06-0.09%, and loss on ignition 8.87-9.86%.

3. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: In step (1), the concentration of citric acid is 1-3 mol / L, and the mass fraction of ammonia water is 36%; In step (1), the mass volume ratio of red mud to citric acid is 5:20-60, in g / mL; In step (1), the acid leaching temperature is 80-83° C., and the acid leaching time is 40-45 min.

4. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: In step (1), the drying temperature is 100-105° C. and the drying time is 24 h. In step (1), the high temperature calcination is carried out by heating the temperature from room temperature to 600-800° C. at a heating rate of 5° C. / min for 2-4 hours.

5. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: In step (2), the mass ratio of the waste thermosetting phenolic resin to the activated red mud catalyst material is 0.5-2:

1.

6. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: The reaction atmosphere during the in-situ catalytic pyrolysis reaction in step (2) is one of nitrogen or argon, and the gas flow rate is 100 mL / min; the temperature is increased to the in-situ catalytic pyrolysis reaction temperature at a heating rate of 10°C / min, the in-situ catalytic pyrolysis reaction temperature is 450-650°C, and the in-situ catalytic pyrolysis reaction time is 20-40 min.

7. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: The waste thermosetting phenolic resin in step (2) is one of waste phenol-type phenolic resin, waste bisphenol A phenolic resin or waste biphenyl aralkyl phenolic resin.

8. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: In step (2), the liquid product in the in-situ catalytic pyrolysis product is an aromatic compound, and the solid product in the in-situ catalytic pyrolysis product is an adsorption material.

9. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: In step (3), the mass ratio of the adsorbent to the volume of the electroplating industrial wastewater containing heavy metals is 2.3-3.0:1, expressed in mg / mL, the adsorption reaction time is 12-24h, and the adsorption reaction temperature is 25-35°C.

10. The method for preparing aromatic compounds and co-producing heavy metal adsorption materials by in-situ catalytic pyrolysis of waste thermosetting phenolic resin from red mud according to claim 1, characterized in that: The heavy metal-containing electroplating industrial wastewater in step (3) has a zinc ion content of ≤50 mg / L, a copper ion content of ≤30 mg / L, and a pH value of 3.0-3.5.

Citation Information

Patent Citations

  • Green cyclic comprehensive utilization method of red mud and lignin waste

    CN111073671A

  • Red mud-based iron-carbon composite material and preparation method and application thereof

    CN113522238A

  • Efficient directional separation method for valuable components of pyrolysis product of waste circuit board

    CN117086078A

  • Method of activation of red mud

    US4017425A

  • Preparation method for and use of magnetic straw biochar material based on red mud enhancement

    WO2024083260A1

Cited By

  • Preparation method and application of modified red mud catalyst

    CN119633826A