Molten glass extrusion molding method
Through the glass liquid extrusion molding method, the pressure extrusion and inflation technology of the extrusion device are used to solve the problem of temperature, fluidity and plasticity balance of glass liquid, which reduces equipment costs and improves process stability. It is suitable for thin glass products Production.
Patent Information
- Application Number
- CN202411022425.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing glass inflation molding technology, the temperature, fluidity and plasticity of the glass liquid are difficult to balance, resulting in high equipment costs and poor process stability, which cannot meet the production needs of finished glass products.
The glass liquid extrusion molding method is adopted. The glass liquid is extruded with pressure instead of gravity through the extrusion device, adjust the speed of the extrusion screw to control the discharge volume, and blow gas into the discharge port to expand to ensure the glass liquid The temperature and fluidity are within the appropriate range.
The controllability and process balance of glass liquid discharge are achieved, equipment costs are reduced, precious metal materials are avoided, and production stability and consistency are improved.
Smart Images

Figure CN118908538A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of glass production, and in particular to a glass liquid extrusion molding method. Background Art
[0002] Glass inflation molding refers to blowing gas into a tubular or annular glass ribbon, using the gas pressure to expand the glass ribbon, thereby making the glass ribbon thinner. During glass inflation molding, the high-temperature glass liquid flows out from the annular discharge port with the help of gravity. In existing inflation molding equipment, the gap of the annular discharge port is generally between 1mm and 5mm. The smaller the gap of the annular discharge port, the thinner the thickness of the glass ribbon / glass liquid that flows out. As the thickness of the finished glass product becomes thinner, the gap of the annular discharge port required is also getting smaller and smaller.
[0003] When the glass liquid needs to flow out of the annular discharge port by gravity, the glass liquid is required to have appropriate fluidity. Therefore, during inflation molding, the fluidity of the molten glass must be increased. Fluidity is related to temperature. Therefore, the temperature of the molten glass needs to be increased to make the fluidity of the glass liquid meet the requirements and flow out naturally under the action of gravity.
[0004] However, as the gap of the annular discharge port becomes smaller and smaller, the temperature of the glass liquid at the annular discharge port will drop significantly; and if the temperature of the glass liquid at the annular discharge port is to meet the requirements, the temperature of the molten glass liquid in the furnace needs to be greatly increased. Only in this way, even if the temperature of the glass liquid at the annular discharge port drops significantly, the temperature and fluidity of the glass liquid at the annular discharge port can be guaranteed. As the temperature of the molten glass liquid increases, the upper temperature limit of the temperature tolerance of the related equipment continues to increase, which makes the existing conventional metal materials (such as high-temperature resistant stainless steel) unable to meet the requirements, and only precious metal materials (such as platinum) can be used. This will cause the cost of equipment to soar.
[0005] In addition, the glass liquid at the annular discharge port needs to have a higher temperature and better fluidity, which is also mutually restricted with the subsequent inflation process. When the temperature and fluidity of the glass liquid increase, the plasticity will decrease, and it will be easy to blow the glass ribbon / glass liquid during inflation, which will reduce the stability of the inflation process and make it difficult to achieve process balance and stability. When the temperature and fluidity of the glass liquid decrease, although the plasticity increases and is conducive to inflation, it is not conducive to flow, and it is difficult to flow out naturally from the annular discharge port, or the outflow rate is difficult to meet the requirements. Therefore, the existing glass discharging process cannot solve the problems between the temperature, fluidity and plasticity of the glass liquid, and it is difficult to balance the differences between the previous and next processes. Therefore, it needs further improvement. Summary of the invention
[0006] The present invention aims to solve the above problems and provides a glass liquid extrusion molding method, which replaces gravity outflow by pressure extrusion, thereby solving the difficult problems between the glass liquid temperature, fluidity and plasticity at the discharge port and balancing the previous and subsequent processes.
[0007] In order to solve the above problems, the present invention provides a glass liquid extrusion molding method, characterized in that it comprises:
[0008] conveying the molten glass to an extrusion device;
[0009] The extrusion device is used to extrude the glass liquid from the annular discharge port.
[0010] Furthermore, before the glass liquid is conveyed to the extrusion device, the temperature of the glass liquid is adjusted to a first temperature, and the first temperature ranges from 900°C to 1200°C.
[0011] Furthermore, when the molten glass is extruded from the annular discharge port or after being extruded, gas is blown into the molten glass extruded from the annular discharge port to cause inflation, so that the molten glass expands and becomes thinner.
[0012] Furthermore, after the glass liquid is transported to the extrusion device,
[0013] Driving the glass liquid to be transported along a first direction in the transport channel;
[0014] The molten glass is squeezed into a mixing channel arranged circumferentially around the transmission channel, so that the molten glass passes through the mixing channel and is squeezed out from the annular discharge port.
[0015] Furthermore, the mixing channel and the transmission channel are isolated and coaxial, and the mixing channel and the transmission channel are connected through a through hole arranged transversely to the first direction.
[0016] Furthermore, a rotatable extrusion screw is provided in the transmission channel, and the extrusion screw is arranged along a first direction, and the glass liquid is driven to be transmitted along the first direction in the transmission channel by the extrusion screw.
[0017] Furthermore, the discharge amount of the annular discharge port is adjusted by adjusting the rotation speed of the extrusion screw.
[0018] Furthermore, the extrusion screw squeezes the molten glass in the transmission channel to drive the molten glass through the mixing channel and to be extruded from the annular outlet.
[0019] Furthermore, the glass liquid is extruded from the annular discharge port along a first direction;
[0020] When gas is blown into the glass liquid extruded from the annular discharge port for expansion, gas is blown into the glass liquid along a first direction at a preset distance from the annular discharge port outside the transmission channel.
[0021] Furthermore, the temperature of the molten glass at the annular discharge port is controlled to be a second temperature, and the second temperature ranges from 750°C to 950°C.
[0022] The beneficial contribution of the present invention is that it effectively solves the above-mentioned problems. The glass liquid extrusion molding method of the present invention replaces gravity outflow by pressure extrusion, so that the glass liquid can be extruded under the action of the extrusion device. In this way, the discharge of the glass liquid is not limited by temperature and fluidity. Even if the temperature and fluidity are reduced, it can be extruded and discharged through the extrusion device. Moreover, the discharge amount can be controlled by controlling the screw speed. In this way, the problem of the temperature, fluidity and plasticity of the glass liquid at the discharge port in the prior art can be solved, so that the front and rear processes can be balanced to achieve process balance and stability. In the glass liquid extrusion molding method of the present invention, the discharge of the glass liquid is no longer strongly related to the temperature, so the glass liquid can be discharged normally by lowering the temperature. The lowering of the temperature of the glass liquid makes the material selection of the glass liquid wider, so that it is not necessary to select precious metal materials (such as platinum) for equipment processing, and conventional high-temperature resistant metal materials (such as high-temperature resistant stainless steel) can also be used, thereby greatly reducing the cost of production equipment. The glass liquid extrusion molding method of the present invention is very innovative, which can greatly reduce the equipment cost and balance the front and back processes of gas expansion, ensuring the process stability and balance, and has strong practicality and should be vigorously promoted. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flow chart of the method of the present invention.
[0024] Figure 2 This is a diagram of the extrusion process after the glass liquid is transported to the extrusion device.
[0025] Figure 3 It is a structural schematic diagram of the extrusion device.
[0026] Figure 4 It is a structural diagram of the die head.
[0027] Figure 5 It is a schematic diagram of the structure of the extrusion screw.
[0028] Figure 6 It is a schematic diagram of the structure of the matrix.
[0029] Figure symbols: base 10, outer shell 11, inner shell 12, first shell 121, second shell 122, spacer 14, inner cover 15, connecting plate 16, die head 20, core 21, joint cavity 211, tapered cavity 2111, straight cavity 2112, plug hole 212, large hole 2121, small hole 2122, connecting part 213, annular convex edge 214, die body 22, discharge port outer mold 221, discharge port inner mold 222, extrusion screw 30, extrusion end 31, middle The spindle hole 33, the straight rod portion 34, the screw portion 35, the positioning portion 36, the joint portion 37, the accommodating cavity 40, the feed port 50, the output port 60, the annular output port 70, the mixing cavity 80, the first cavity portion 81, the first annular wall 811, the second annular wall 812, the top wall 813, the second cavity portion 82, the third annular wall 821, the fourth annular wall 822, the third cavity portion 83, the fifth annular wall 831, the sixth annular wall 832, the through hole 90, the first direction Y, the second direction X, and the first path S. DETAILED DESCRIPTION
[0030] The following examples are provided to further explain and supplement the present invention and do not constitute any limitation to the present invention.
[0031] like Figure 1-2 As shown, the main point of the glass liquid extrusion molding method of the present invention is that the glass liquid is extruded from the annular discharge port by an extrusion device, and pressure extrusion is used instead of gravity flow, thereby solving the problems existing in the existing process.
[0032] The glass liquid extrusion molding device of the present invention comprises the following steps:
[0033] conveying the molten glass to an extrusion device;
[0034] The extrusion device is used to extrude the glass liquid from the annular discharge port.
[0035] Before the glass liquid is conveyed to the extrusion device, the temperature of the glass liquid is adjusted to a first temperature, wherein the first temperature ranges from 900°C to 1200°C.
[0036] During processing, the glass raw materials are first heated and melted to form high-temperature glass liquid. At this time, the temperature of the glass liquid is a third temperature, which is different from the first temperature. Usually, the third temperature is greater than the first temperature, and the third temperature ranges from 1200°C to 1600°C.
[0037] When the glass raw materials are heated to form glass liquid at the third temperature, the glass liquid is adjusted to the first temperature by a certain method. The adjustment method is not limited. For example, the temperature of the glass liquid can be lowered by passing the glass liquid through a certain cooling channel, so that the temperature drops from the third temperature to the first temperature. The cooling channel generally refers to a channel that can lower the temperature of the glass liquid. When the temperature of the glass liquid drops through the cooling channel, it can be naturally cooled or accelerated cooling by a cooling medium. Normally, when no additional heat source is provided to the glass liquid to maintain its temperature, the glass liquid will directly or indirectly exchange heat with the outside to cool down. Therefore, by allowing the glass liquid to flow naturally through a certain path, cooling can be achieved, so that its temperature drops from the third temperature to the first temperature.
[0038] When the temperature of the glass liquid is adjusted to the first temperature, the glass liquid can be transported to the extrusion device.
[0039] After the molten glass at the first temperature is delivered to the extrusion device, the molten glass extrusion molding method of the present invention further comprises the following steps:
[0040] Driving the glass liquid to be transported along a first direction in the transport channel;
[0041] The molten glass is squeezed into a mixing channel arranged circumferentially around the transmission channel, so that the molten glass passes through the mixing channel and is squeezed out from the annular discharge port.
[0042] In the above steps, the transmission channel and the mixing channel are both arranged on the extrusion device. The mixing channel and the transmission channel are isolated and coaxially arranged. The mixing channel and the transmission channel are connected through a through hole arranged transversely to the first direction.
[0043] The extrusion device drives the glass liquid to be transported in the transmission channel along the first direction, and squeezes the glass liquid into the mixing channel of the extrusion device through the through hole, and finally extrude it from the annular outlet through the mixing channel.
[0044] Furthermore, the annular discharge port is arranged on the extrusion device, which is the outlet of the mixing channel.
[0045] In order to drive the glass liquid to be transported along the first direction in the transport channel, a rotatable extrusion screw is provided in the transport channel. The extrusion screw is arranged along the first direction, and the glass liquid can be driven to be transported along the first direction in the transport channel by the extrusion screw.
[0046] The structure of the extrusion screw is not limited, as long as it can drive the glass liquid to be transported along the first direction.
[0047] The force exerted by the extrusion screw on the molten glass also drives the molten glass to pass through the mixing channel and be extruded from the annular outlet.
[0048] In other words, the extrusion screw directly acts on the molten glass in the transmission channel to drive the molten glass to be transmitted along the first direction, and the force of the extrusion screw is transmitted through the molten glass and indirectly applied to the molten glass in the mixing channel, so that the molten glass in the mixing channel is also driven to be extruded from the annular discharge port.
[0049] The glass liquid is squeezed out from the annular discharge port by an extrusion screw, so that the discharge of the glass liquid no longer depends on gravity and fluidity. Even if the temperature of the glass liquid is low and the fluidity is poor, the glass liquid can still be squeezed out for discharge. In this way, the mutual restriction problem between the high temperature, fluidity and plasticity of the glass liquid can be solved. Extrusion through an extrusion screw can make the discharge controllable, so that the discharge is no longer strongly related to the temperature, and thus achieve process balance and stability.
[0050] Since the discharge of the glass liquid depends on the extrusion screw, the discharge amount of the annular discharge port can be adjusted by adjusting the speed of the extrusion screw. More specifically, the discharge flow rate of the annular discharge port, that is, the total amount of glass liquid flowing out of the annular discharge port per unit time, can be adjusted by adjusting the speed of the extrusion screw.
[0051] Extruding the glass liquid through the transmission channel first and then through the mixing channel is conducive to eliminating the influence of the movement of the extrusion screw on the discharge. When the extrusion screw is working, the extrusion screw rotates around a fixed axis. In theory, the fixed axis is the central axis of the extrusion screw. However, in practice, when the extrusion screw is working, the central axis of the extrusion screw will be offset. If the annular discharge port is set to be directly connected to the transmission channel, the rotation of the extrusion screw will affect the discharge of the annular discharge port, resulting in uneven thickness of the discharged glass liquid. When the subsequent process is bulged, it is easy to produce streak defects. Setting a mixing channel to introduce the glass liquid into the mixing channel, the mixing channel and the extrusion screw are located in different spaces, and the two are relatively isolated, so that the influence of the rotation of the extrusion screw on the discharge can be eliminated; after the glass liquid passes through the mixing channel with a relatively fixed shape and size, it is extruded from the annular discharge port, which can ensure tolerance and concentricity, thereby avoiding streak defects when the glass is bulged, and ensuring process stability and consistency.
[0052] When the molten glass is extruded from the annular discharge port, the molten glass is extruded along a first direction.
[0053] In order to ensure the balance of the previous and next processes, the temperature of the glass liquid at the annular discharge port is controlled to be a second temperature. The temperature of the second temperature is lower than the first temperature, and the range of the second temperature is 750°C to 950°C.
[0054] The second temperature having a temperature range smaller than the first temperature means, for example, that when the first temperature range is 900°C, the second temperature is smaller than 900°C and greater than or equal to 750°C.
[0055] When the glass liquid is extruded from the annular discharge port or after being extruded, gas is blown into the glass liquid extruded from the annular discharge port to expand the glass liquid, so that the glass liquid expands and becomes thinner.
[0056] When the glass liquid is extruded from the annular discharge port, it may form an annular glass liquid with a hollow interior, or it may form a solid columnar glass liquid with a collection of interior parts. By setting the air blowing point inside the glass liquid, air can be expanded from inside the glass liquid, causing the glass liquid to expand and become thinner.
[0057] In order to prevent the glass liquid from expanding and touching the extrusion device where the annular outlet is located, when gas is blown into the glass liquid for expansion, gas is blown into the glass liquid along the first direction outside the transmission channel at a preset distance from the annular outlet.
[0058] The gas is introduced into the interior of the glass liquid along the first direction for expansion. Preferably, the gas is introduced into the interior of the glass liquid along the first direction through the central axis of the extrusion screw. In this way, when the gas passes through the interior of the extrusion screw, it can take away part of the heat and cool the glass liquid in the transmission channel, and it is beneficial to increase the life of the extrusion screw. Similarly, when the gas passes through the extrusion screw, the gas will also be heated. When it enters the interior of the glass liquid, it is also beneficial to provide a certain amount of heat for the glass liquid to prevent the temperature of the glass liquid from dropping too quickly and hardening after extrusion.
[0059] The gas is introduced into the glass liquid along the first direction, which means that the direction in which the gas is transmitted to the glass liquid is along the first direction, and does not mean that the gas can only be blown out along the first direction inside the glass liquid.
[0060] In fact, when the gas is blown out from the glass liquid, it may be along the first direction or along other directions. For example, a trumpet-shaped expansion structure is provided at the end of the gas passage for conveying the gas, so that the direction of the gas blowing out can be changed. At this time, the actual blowing direction of the gas is no longer the first direction, but it still belongs to the gas passing into the glass liquid along the first direction as described in the present application.
[0061] Furthermore, in order to facilitate the blowing of gas into the glass liquid at a preset distance from the annular discharge port outside the transmission channel, an extended air channel can be provided. The extended air channel is provided along the first direction and is coaxial with the central axis of the extrusion screw. The extended air channel extends to a certain length outside the extrusion device, and the interior of the extended air channel is connected with the interior of the extrusion screw to form an air channel extending along the first direction. In this way, gas can be blown into the glass liquid at a preset distance from the annular discharge port through the air channel.
[0062] When the gas is blown into the molten glass, the molten glass expands under the action of the gas pressure, thereby reducing its thickness, thereby forming a thin tubular glass ribbon.
[0063] The tubular glass ribbon is then passed through a roller press to be flattened into a flat tubular glass ribbon; the tubular glass ribbon is then trimmed to separate the tubular glass ribbon into two long strips of glass ribbon. Then, the cutting, winding and other processes can be performed according to the existing technology to form the desired ultra-thin glass.
[0064] For the present invention, the specific structure of the extrusion device is not limited, as long as it can achieve the functions described in the present invention. The main point of the present invention is that the glass liquid can be extruded from the annular discharge port by pressure extrusion of the extrusion device, and the pressure extrusion replaces the traditional gravity outflow. Because the temperature of the glass liquid has been adjusted to the first temperature before the glass liquid is transported to the extrusion device, and the temperature of the glass liquid at the annular discharge port is controlled to the second temperature, the extrusion device can adapt to the temperature of the glass liquid.
[0065] In order to more clearly describe the technical solution of the present invention, the structure of the extrusion device of this embodiment is specifically described below. It should be understood that the extrusion device is not limited to the following specific structure:
[0066] Benru Figure 3 to Figure 6 As shown, the main point of the glass liquid extrusion device of the invention is that the glass liquid is extruded from the annular discharge port 70 by the extrusion screw 30, and the pressure extrusion replaces the traditional gravity outflow, thereby solving the mutual restriction problem between the high temperature and fluidity of the molten glass liquid and the plasticity of the glass after discharge. Extrusion through the extrusion screw 30 can make the discharge controllable, so that the discharge amount is no longer strongly related to the temperature, so that the discharge amount can be changed by changing the screw speed under the condition of reducing or keeping the temperature constant, thereby achieving process balance and stability.
[0067] The glass liquid extrusion device of the present invention comprises a base body 10, a die head 20, an extrusion screw 30 and a power unit. Among them, the base body 10 is provided with a cavity 40 that can accommodate high-temperature glass liquid, and the cavity 40 forms the transmission channel in the above method. The base body 10 is provided with a feed port 50 and an output port 60, the feed port 50 is used to transport the glass liquid into the cavity 40, and the output port 60 is used for extruding the glass liquid. The feed port 50 and the output port 60 are respectively connected with the cavity 40. The die head 20 is connected to the output port 60 of the base body 10, and the extrusion screw 30 is arranged in the cavity 40. An annular discharge port 70 for the glass liquid to flow out is provided between the extrusion end 31 of the extrusion screw 30 and the die head 20 or on the die head 20, and the extrusion screw 30 can extrude the glass liquid from the annular discharge port 70. The power unit is connected to the driving end of the extrusion screw 30 , and is used to drive the extrusion screw 30 to rotate in the cavity 40 to extrude the glass liquid from the annular discharge port 70 .
[0068] During operation, the glass liquid is transported to the cavity 40 of the substrate 10 through the feed port 50; the temperature of the glass liquid transported to the cavity 40 does not need to reach the high temperature of the conventional molten glass liquid, and the temperature of the glass liquid can be controlled within the first temperature range. In this embodiment, the first temperature range is 900° to 1200°. When the temperature of the molten glass liquid is controlled within the first temperature range in the previous process, it can be transported to the cavity 40 of the substrate 10 through the feed port 50.
[0069] Since the temperature of the glass liquid contained in the base 10 is within the first temperature range and has not reached the melting temperature of traditional glass liquid, the base 10 can be made of non-precious metal materials, such as stainless steel and corundum tube materials, without having to use precious platinum materials or build a kiln with refractory bricks. In this way, the material selection range of the base 10 can be expanded and the cost of production equipment can be greatly reduced.
[0070] When the glass liquid at the first temperature enters the cavity 40 of the base 10 , the extrusion screw 30 is driven by the power unit to rotate, thereby driving the glass liquid to be transported and extruded along the direction of the annular discharge port 70 .
[0071] When the first direction Y is horizontal, the molten glass cannot be transported along the direction of the output port 60 under the action of gravity. At this time, the molten glass is basically transported forward by the extrusion screw 30 .
[0072] When the first direction Y is not horizontal, especially when the first direction Y is vertical, the molten glass can flow toward the outlet 60 under the action of gravity. However, the molten glass is mainly transported forward by the extrusion screw 30, and gravity only helps the flow.
[0073] Since the transmission of the glass liquid to the output port 60 mainly depends on the rotation of the extrusion screw 30, and does not necessarily rely on gravity and fluidity, the discharge amount can be adjusted by adjusting the speed of the extrusion screw 30. In the traditional process, the discharge must rely on the gravity of the glass liquid, and the fluidity of the glass liquid must reach a certain level when discharging, and the fluidity is affected by temperature. Therefore, the discharge must have a very high temperature and fluidity; and the present application is extruded by the extrusion screw 30, which replaces the gravity outflow with pressure extrusion. Even if the fluidity of the glass liquid is poor, it can be extruded under the action of the extrusion screw 30. In this way, the discharge can be controlled, and it is not necessary to adjust the fluidity of the glass liquid by adjusting the temperature of the glass liquid, so that the discharge of the glass liquid is no longer strongly related to the temperature. The present invention can change the discharge amount by changing the speed of the extrusion screw 30 under the condition of reducing or maintaining a constant temperature, and the temperature of the glass liquid can be reduced to a second temperature for discharge. The range of the second temperature is 750°~950°. Among them, the second temperature refers to the temperature of the glass liquid at the annular discharge port 70.
[0074] By extruding the glass liquid through the extrusion screw 30, the mutual restriction problem between the high temperature of the melting temperature, the fluidity and the plasticity of the glass after discharge can be solved. Because the extrusion through the extrusion screw 30 does not necessarily require the glass liquid to be at a high temperature to have good fluidity, it can also be extruded at a lower temperature. The glass liquid at a lower temperature is more suitable for the subsequent blowing process, thereby ensuring the stability of the blowing process and achieving process balance and stability.
[0075] In some embodiments, the extrusion end 31 of the extrusion screw 30 is disposed in the die head 20, and the die head 20 has an opening, and an annular discharge port 70 is formed between the opening of the die head 20 and the extrusion end 31. This embodiment has a simple structure and smoother material mixing, but since the extrusion screw 30 is a rotating component, there will be displacement deviation during rotation, which will cause a large tolerance of the annular discharge port 70, which brings uncontrollable factors to the stability of the subsequent inflation process.
[0076] In some embodiments, in order to adjust the tolerance of the annular discharge port 70 and eliminate the unstable factors caused by the rotation of the extrusion screw 30, a mixing chamber 80 is provided in the die head 20, and the mixing chamber 40 forms the mixing channel in the above method. The mixing chamber 80 is connected with the containing chamber 40 through the through hole 90, so that when the extrusion screw 30 rotates, the glass liquid is squeezed into the mixing chamber 80 through the through hole 90, and then discharged from the mixing chamber 80. In this way, the discharge can be isolated from the extrusion screw 30, the unstable factors caused by the rotation of the extrusion screw 30 are eliminated, and the gap tolerance of the annular discharge port 70 is guaranteed, so as to avoid the stripe defect of the glass liquid due to the uneven thickness of the discharge in the subsequent inflation process.
[0077] The mixing chamber 80 is circumferentially arranged around the extrusion end 31, and the mixing chamber 80 extends along the first path S and penetrates to the end of the die head 20, thereby forming the annular discharge port 70 at the end of the die head 20. In the absence of the through hole 90, the mixing chamber 80 is isolated from the cavity 40 where the extrusion screw 30 is located; the mixing chamber 80 and the cavity 40 are penetrated by the through hole 90.
[0078] The through hole 90 is provided on the die head 20. The through hole 90 penetrates the containing cavity 40 and the mixing cavity 80 in a direction transverse to the first direction Y. In the present embodiment, the through hole 90 is perpendicular to the first direction Y. The number of the through holes 90 is not limited, and at least one through hole 90 is provided. When a plurality of through holes 90 are provided, the through holes 90 are preferably arranged at uniform intervals along the circumferential direction. The size of the through hole 90 can be adjusted as required, and it is a small hole relative to the size of the containing cavity 40 and the mixing cavity 80. The shape of the through hole 90 can be set as required. Preferably, the through hole 90 is set as a circular hole, which can eliminate stress and avoid bubbles in the glass liquid.
[0079] The first path S is inclined or curved relative to the first direction Y. The first path S may be a straight path or a curved path. In this embodiment, the first path S is set as a curved path.
[0080] The size of the mixing chamber 80 in the second direction X transverse to the first direction Y is reduced along the first path S. When viewed along the first path S, the size of the mixing chamber 80 is reduced. The reduction includes linear reduction and nonlinear reduction. In this embodiment, the size of the mixing chamber 80 is nonlinearly reduced along the first path S.
[0081] Furthermore, the mixing chamber 80 includes a first chamber portion 81 , a second chamber portion 82 , and a third chamber portion 83 which are connected to each other.
[0082] The first cavity 81 includes a first annular wall 811, a second annular wall 812, and a top wall 813. The first annular wall 811 and the second annular wall 812 are spaced apart from each other and are arranged around the extrusion end 31 in the circumferential direction. The diameter of the first annular wall 811 is greater than the diameter of the second annular wall 812. The top wall 813 is connected to one end of the first annular wall 811 and the second annular wall 812 away from the second cavity 82, and the top is arched, which is arched in the direction away from the second cavity 82. The space enclosed by the first annular wall 811, the second annular wall 812, and the top wall 813 is the first cavity 81.
[0083] In order to guide the flow of the glass liquid and avoid the generation of bubbles in the glass liquid, the second annular wall 812 is inclined, and is inclined in a direction away from the central axis of the extrusion screw 30. The through hole 90 is provided on the second annular wall 812, and more specifically, the through hole 90 is provided at one end of the second annular wall 812 close to the top wall 813, so that when the glass liquid is squeezed into the mixing chamber 80 through the through hole 90, the glass liquid will flow along the second annular wall 812. By guiding the flow of the glass liquid through the second annular wall 812, it is possible to avoid the generation of bubbles in the glass liquid due to the mixing of air when the glass liquid sags naturally.
[0084] The first annular wall 811 is parallel or approximately parallel to the first direction Y as a whole.
[0085] To eliminate stress and avoid bubble generation, the connection between the first annular wall 811 and the top wall 813, and the connection between the second annular wall 812 and the top wall 813 should be rounded, so that the wall surface of the first cavity 81 is curved without sharp turns or sharp protrusions.
[0086] The second cavity 82 includes a third annular wall 821 and a fourth annular wall 822 which are spaced apart from each other. The third annular wall 821 and the fourth annular wall 822 are both arranged around the extrusion end 31 in the circumferential direction. The third annular wall 821 is connected to the first annular wall 811, and the fourth annular wall 822 is connected to the second annular wall 812. The second cavity 82 is formed between the third annular wall 821 and the fourth annular wall 822. The diameter of the third annular wall 821 is greater than the diameter of the fourth annular wall 822. The third annular wall 821 and the fourth annular wall 822 are arranged obliquely, and are inclined in a direction of approaching relative to the central axis of the extrusion screw 30. Observed from the first path S, the second cavity 82 is getting closer and closer to the central axis of the extrusion screw 30.
[0087] Furthermore, the third annular wall 821 and the fourth annular wall 822 have different inclinations, so that the distance between the third annular wall 821 and the fourth annular wall 822 is reduced along the first path S, thereby reducing the flow rate of the molten glass, which is beneficial to thinning the molten glass.
[0088] Similarly, the connection between the first annular wall 811 and the third annular wall 821, and the connection between the second annular wall 812 and the fourth annular wall 822 are both rounded transitions, so that the wall surface of the mixing chamber 80 is curved without sharp turns or sharp protrusions.
[0089] The third cavity 83 includes a fifth annular wall 831 and a sixth annular wall 832 which are spaced apart from each other. The fifth annular wall 831 and the sixth annular wall 832 are arranged circumferentially around the extrusion end 31. The fifth annular wall 831 is connected to the third annular wall 821, and the sixth annular wall 832 is connected to the fourth annular wall 822. The third cavity 83 is formed between the fifth annular wall 831 and the sixth annular wall 832. The fifth annular wall 831 and the sixth annular wall 832 are arranged in a nearly parallel direction relative to the central axis of the extrusion screw 30, so that the flow rate of the glass liquid in the third cavity 83 is stable, and the glass liquid is more stable when flowing out of the annular discharge port 70, thereby further ensuring the stability of the subsequent inflation process.
[0090] Similarly, the connection between the third annular wall 821 and the fifth annular wall 831, and the connection between the fourth annular wall 822 and the sixth annular wall 832 are both rounded transitions, so that the wall surface of the mixing chamber 80 is curved without sharp transitions or sharp protrusions.
[0091] When the glass liquid enters the mixing chamber 80 through the through hole 90, it flows along the first path from the first chamber portion 81 through the second chamber portion 82 to the third chamber portion 83, and finally flows out from the annular outlet 70. When the glass liquid flows downward in the mixing chamber 80, relative to the central axis, the glass liquid flows downward in a slightly spiral direction along the circumferential direction.
[0092] Furthermore, for the convenience of assembly, the die head 20 includes a core 21 and a body 22. The core 21 is connected to the output port 60, and the body 22 is sleeved outside the core 21 and fixedly connected to the core 21 and / or the base 10. The mixing cavity 80 is formed between the inner wall of the body 22 and the outer wall of the core 21. The mixing cavity 80 can be formed by the core 21 and the body 22 components. In order to form the mixing cavity 80, a concave structure with a corresponding shape should be provided on the outer wall of the core 21 and the inner wall of the body 22, and the two are matched to form the mixing cavity 80.
[0093] The mold core 21 is provided with a joining cavity 211 and a plug hole 212 which are arranged to penetrate along the first direction Y. The opening of the joining cavity 211 faces the containing cavity 40, and it is connected with and penetrates the containing cavity 40. The through hole 90 is provided on the joining cavity 211, and the through hole 90 directly penetrates the joining cavity 211 and the mixing cavity 80, so that the glass liquid in the containing cavity 40 can be transported to the mixing cavity 80 through the joining cavity 211 and the through hole 90.
[0094] The engaging cavity 211 is used to form a joint with the extrusion end 31 of the extrusion screw 30 to seal the output port 60, which is beneficial to process control. During implementation, the extrusion screw 30 can be controlled to move axially to engage with or disengage from the engaging cavity 211. For example, during the initial production period, the extrusion screw 30 can be moved axially toward the engaging cavity 211 so that the base screw 30 and the engaging cavity 211 are shaped and sealed to seal the output port 60. In this way, the glass liquid will be collected in the cavity 40 after entering the cavity 40. At this time, the temperature of each component can be increased by the high temperature of the glass liquid. When the glass liquid is collected in the cavity 40 to a certain amount and the temperature of each component also rises, the extrusion screw 30 can be controlled to move axially away from the engaging cavity 211 to disengage, thereby opening the output port 60, so that the glass liquid can be squeezed into the mixing cavity 80 under the action of the extrusion screw 30, and finally flow out from the annular outlet 70.
[0095] The extrusion end 31 of the extrusion screw 30 is inserted into the insertion hole 212 and can rotate in the insertion hole 212 to extrude the glass liquid in the joining cavity 211 into the mixing cavity 80 through the through hole 90 , so that the glass liquid can be discharged from the annular discharge port 70 .
[0096] The engaging cavity 211 and the inserting hole 212 penetrate the mold core 21 , and a step structure is formed between the engaging cavity 211 and the inserting hole 212 . More specifically, the engaging cavity 211 includes a tapered cavity portion 2111 and a straight cavity portion 2112 .
[0097] The opening diameter of the tapered cavity 2111 is consistent with the diameter of the containing cavity 40 , and is connected to the output port 60 of the base 10 . The tapered cavity 2111 is in a tapered shape with a gradually narrowing opening, and is used for shape engagement with the extrusion screw 30 .
[0098] The straight cavity 2112 is disposed at the constricted end of the tapered cavity 2111, and its diameter is smaller than the diameter of the receiving cavity 40. The through hole 90 is disposed on the wall of the straight cavity 2112.
[0099] The plug hole 212 is a stepped hole, which includes a large hole portion 2121 and a small hole portion 2122. The diameter of the large hole portion 2121 is larger than the diameter of the small hole portion 2122, and smaller than the diameter of the straight cavity portion 2112. The large hole portion 2121 is disposed between the straight cavity portion 2112 and the small hole portion 2122, so that a stepped structure is formed between the straight cavity portion 2112, the large hole portion 2121, and the small hole portion 2122.
[0100] The extrusion end 31 of the extrusion screw 30 is inserted into the large hole portion 2121 and can rotate in the large hole portion 2121. The coaxiality of the extrusion screw 30 can be ensured by the large hole portion 2121.
[0101] In order to facilitate the connection between the base body 10 and the mold core 21, a stepped annular groove is provided at the bottom end of the base body 10, and the mold core 21 is provided with a cylindrical connecting portion 213 and an annular convex edge 214 protruding from the circumferential surface of the connecting portion. The connecting portion 213 and the annular convex edge 214 are embedded in the annular groove, and the mold core 21 is axially limited by the mold body 22, so that the mold core 21 is clamped between the base body 10 and the mold body 22 and is in a fixed state.
[0102] Further, the mold body 22 includes an outlet outer mold 221 and an outlet inner mold 222 that are connected in a first direction Y. The outlet inner mold 222 is shaped to be engaged in the outlet outer mold 221, and the mixing cavity 80 is formed between the inner walls of the outlet outer mold 221 and the outlet inner mold 222 and the outer wall of the mold core 21.
[0103] Specifically, a concave receiving groove is provided on the end surface of the discharge port outer mold 221. The shape of the receiving groove is basically matched with the outer wall shape of the discharge port inner mold 222, but may have a certain tolerance. The discharge port inner mold 222 may be engaged in the receiving groove. In this embodiment, the receiving groove is a circular groove.
[0104] Concave structures corresponding to the mixing cavity 80 are formed on the inner walls of the discharge port inner mold 222 and the discharge port outer mold 221 , respectively, and are matched with the outer wall of the mold core 21 to form the mixing cavity 80 .
[0105] By setting the discharge port inner mold 222 and the discharge port outer mold 221, it is convenient to adjust the shape and size of the mixing cavity 80 by replacing the discharge port inner mold 222, so as to adjust the size of the annular discharge port 70, and facilitate structural processing and assembly. In addition, it is also convenient to adjust the tolerance and coaxiality of the annular discharge port 70 by fine-tuning the position of the discharge port inner mold 222 relative to the discharge port outer mold 221. During implementation, a strip hole or a plurality of optional holes can be set on the discharge port inner mold 222, and the discharge port inner mold 222 is connected to the discharge port outer mold 221 through fasteners installed in the strip hole, so that the position of the discharge port inner mold 222 relative to the discharge port outer mold 221 can be fine-tuned to adjust the gap tolerance of the annular discharge port 70. Or the position of the discharge port inner mold 222 relative to the discharge port outer mold 221 can be adjusted by fixing through different optional holes as needed.
[0106] The discharge port outer mold 221 is block-shaped as a whole, and is attached to the end of the base 10 to fix the mold core 21. The discharge port outer mold 221, the discharge port inner mold 222, and the base 10 can be fastened by screws.
[0107] Furthermore, to facilitate gas expansion, the extrusion screw 30 is provided with a central axis hole 33 that passes through both ends along its central axis. The central axis hole 33 forms a gas transmission channel. The central axis hole 33 is aligned with the plug hole 212. Specifically, the central axis hole 33 passes through the small hole portion 2122 of the plug hole 212, and the diameter of the central axis hole 33 is consistent with or close to the diameter of the small hole portion 2122. When the glass liquid flows out from the annular discharge port 70, gas can be input into the glass liquid through the central axis hole 33 for gas expansion. The gas expansion refers to blowing air into the annular glass liquid (or glass ribbon) so that the glass liquid (glass ribbon) expands under the action of air pressure, thereby making the thickness of the glass liquid (glass ribbon) thinner, and then forming the desired ultra-thin glass through subsequent processes. In addition, when gas is transmitted through the central axis hole 33, part of the heat can be taken away to cool the extrusion screw 30, thereby increasing the life of the extrusion screw 30.
[0108] Furthermore, the glass liquid extrusion device of the present invention also includes a stabilizing rod. The stabilizing rod is in the shape of a cylindrical tube, one end of which is inserted into the central axis hole 33, and the other end extends out of the die head 20. The interior of the stabilizing rod is connected to the central axis hole 33, and the gas input into the central axis hole 33 can be blown out through the stabilizing rod. The stabilizing rod is used to extend the gas transmission channel, so that the gas can be introduced into the interior of the glass liquid at a certain distance from the annular discharge port 70 for inflation, rather than being blown out directly from the bottom of the die head for inflation. The stabilizing rod provides the extended airway.
[0109] The centering rod is fixedly connected to the extrusion screw 30 , and the fixed connection method thereof includes but is not limited to fixing the centering rod in the central axis hole 33 in an interference fit manner.
[0110] Furthermore, the extrusion screw 30 sequentially includes a straight rod portion 34, a screw portion 35, a joint portion 37, and a positioning portion 36. The straight rod portion 34 is in the shape of a long rod, and its outer wall is a circumferential wall surface, which is arranged in the cavity 40; one end of the straight rod portion 34 can extend out of the base 10 to form the driving end.
[0111] The screw portion 35 is provided with an extrusion thread, which is arranged in the housing 40. The positioning portion 36 is inserted into the insertion hole 212 and can rotate in the insertion hole 212. The central axis hole 33 passes through the straight rod portion 34, the screw portion 35, the joint portion 37 and the positioning portion 36 along the length direction.
[0112] One end of the straight rod portion 34 opposite to the positioning portion 36 is the driving end of the extrusion screw 30 , which is used to be connected to the power unit so that it can rotate under the drive of the power unit.
[0113] The positioning portion 36 is cylindrical, and cooperates with the large hole portion 2121 and can rotate in the large hole portion 2121. The positioning portion 36 is spaced a certain distance from the through hole 90 to provide space for the glass liquid. In this embodiment, one end of the positioning portion 36 abuts against the large hole portion 2121, and the other end extends out of the large hole portion 2121 and is spaced coaxially with the straight cavity portion 2112.
[0114] The engaging portion 37 is located in the engaging cavity 211. The end of the engaging portion 37 close to the positioning portion 36 is provided with a conical surface. The engaging portion 37 can be pressed against the wall of the conical cavity 2111 by its conical surface, thereby forming a shape engagement and sealing the output port 60. By controlling the extrusion screw 30 to move axially toward the plug hole 212, the engaging portion 37 can be controlled to fit with the conical cavity 2111 to form a shape engagement. By controlling the extrusion screw 30 to move axially away from the plug hole 212, the engaging portion 37 can be controlled to separate from the conical cavity 2111 to open the output port 60.
[0115] When the output port 60 is not sealed, when the extrusion screw 30 rotates, the glass liquid is transported along the direction of the joining chamber 211 driven by the screw portion 35, enters from the conical chamber portion 2111 to the straight chamber portion 2112, and then is extruded from the through hole 90 to the mixing chamber 80, and finally discharged from the annular discharge port 70 of the mixing chamber 80.
[0116] When the glass liquid enters the straight cavity portion 2112, even if the glass liquid enters the plug-in hole 212, due to the low temperature at the bottom of the plug-in hole 212, the fluidity of the glass liquid will decrease after entering and it will be unable to flow out from the plug-in hole 212 further. Moreover, the glass liquid with low fluidity itself can play a sealing role. Therefore, the extrusion end 31 of the extrusion screw 30 rotates in the plug-in hole 212 and does not affect the normal discharge of the glass liquid. The glass liquid will not actually be discharged from the small hole portion 2122 of the plug-in hole 212.
[0117] Moreover, when gas is introduced into the central axis hole 33 of the extrusion screw 30, it is beneficial to reduce the temperature of the extrusion screw 30, which can also reduce the temperature of the extrusion end 31, so that even if the glass liquid flows into the plug hole 212, it will be cooled at the plug hole 212 and the fluidity will deteriorate, and thus it will be impossible to discharge from the small hole portion 2122.
[0118] Further, the base 10 includes an outer shell 11 and an inner shell 12 which are coaxial and spaced apart from each other. Further, it may also include a supporting cylinder. The central axes of the outer shell 11, the inner shell 12 and the supporting cylinder are arranged along the first direction Y.
[0119] The outer shell 11 is sleeved outside the inner shell 12, and both are cylindrical. The outer shell 11 and the inner shell 12 are coaxially spaced to form a heat-insulating structure, which is beneficial to heat preservation of the internal cavity 40 of the base 10 and reduces heat loss. The interior of the inner shell 12 forms the cavity 40 for containing the glass liquid at the first temperature.
[0120] In order to make the outer shell 11 and the inner shell 12 coaxially spaced, a spacer 14 is provided between the ends of the outer shell 11 and the inner shell 12. The spacer 14 is provided between the outer shell 11 and the inner shell 12 and fits with the inner wall of the outer shell 11 and the outer wall of the inner shell 12.
[0121] The support cylinder is arranged in the inner shell 12, and is spaced apart from the inner shell 12. In order to make the cavity 40 relatively closed, an inner cover 15 is provided at one end of the inner shell 12 away from the die head 20. The inner cover 15 can close the end of the inner shell 12. In this embodiment, the inner cover 15 is integrally formed with the spacer 14 at the end, and the inner cover 15 covers the end of the inner shell, and the outer shell 11, the spacer 14 and the inner shell 12 are fastened by screws.
[0122] The straight rod portion 34 and the screw portion 35 of the extrusion screw 30 are disposed in the housing 40. When the base 10 is provided with a support cylinder, the straight rod portion 34 is inserted into the support cylinder, so that the straight rod portion 34 can be protected by the support cylinder and the extrusion screw 30 can be supported.
[0123] The length of the support cylinder in the inner shell 12 should be shorter than the length of the inner shell 12, so that the straight rod portion 34 of the extrusion screw 30 is inserted into the support cylinder, and the screw portion 35 is located outside the support cylinder and inside the inner shell 12. The support cylinder is mainly used to protect the extrusion screw 30. Although the straight rod portion 34 of the extrusion screw 30 can withstand high temperatures, it will be deformed to a certain extent when it is in a high temperature environment of glass liquid for a long time. A support cylinder is set outside the straight rod portion 34, and the straight rod portion 34 can be protected by temperature isolation using the support cylinder. The support cylinder can be made of a corundum tube.
[0124] Furthermore, one end of the support cylinder away from the screw portion 35 extends out of the inner shell 12 , and correspondingly, the straight rod portion 34 also extends out of the inner shell 12 and is connected to the power portion.
[0125] Further, the feed port 50 is transverse to the first direction Y. Specifically, corresponding through holes are respectively provided on the outer shell 11 and the inner shell 12, and the through holes form the feed port 50. By connecting a tubular component at the feed port 50, the glass liquid can be transported to the cavity 40 through the feed port 50.
[0126] Furthermore, the feed port 50 is disposed on the base body 10 at a position corresponding to the straight rod portion 34 and close to the screw rod portion 35 .
[0127] The axial direction of the output port 60 is parallel to the first direction Y. In this embodiment, the end of the inner shell 12 forms the output port 60 .
[0128] Further, to save costs, the inner shell 12 includes a first shell 121 and a second shell 122 that are butt-jointed along a first direction Y. The first shell 121 and the second shell 122 are made of materials with different temperature resistance limits. The second shell 122 is located between the first shell 121 and the die head 20 .
[0129] In this embodiment, the feed port 50 is located on the second shell portion 122 , so that the molten glass first enters into the second shell portion 122 .
[0130] For the entire glass liquid extrusion device, the temperature at the feed port 50 is the highest. After the glass liquid enters the cavity 40, the temperature of the glass liquid in the cavity 40 will drop slightly, and the temperature of the glass liquid at the annular discharge port is the lowest. Therefore, for the entire substrate 10, the second shell 122 bears the highest glass liquid temperature, so it can be processed with a first material with high temperature resistance. The temperature of the first shell 121 and the outer shell 11 is lower than that of the second shell 122, so it can be processed with a second material with slightly lower temperature resistance. The temperature resistance limit of the first material is greater than the temperature resistance limit of the second material. For example, the first material can be a corundum tube, and the second material can be a high-temperature resistant stainless steel material. Under the same circumstances, the cost of a material with high temperature resistance will be higher. By setting the inner shell 12 and the outer shell 11 with coaxial spacing, and setting the inner shell 12 to be connected by the first shell 121 and the second shell 122, the substrate 10 can be processed with materials of different costs, and it is not necessary to use all materials with the best temperature resistance for processing, thereby greatly reducing the material cost.
[0131] In some embodiments, the feed port 50 may also be disposed on the first shell portion 121 , the first shell portion 121 is processed using a first material, and the second shell portion 122 is processed using a second material.
[0132] Further, in order to facilitate the fixed connection between the base 10 and the die head 20, a connecting plate 16 is provided at one end of the outer shell 11 and the inner shell 12 close to the die head 20. The connecting plate 16 is integrally formed with the spacer 14 at the end. The connecting plate 16 abuts between the outer shell 11 and the die head 20 and is fixedly connected by screws.
[0133] In the present application, the base 10 is a tubular component, and its components are molded from heat-resistant materials and then assembled to form the base 10. The base 10 is not made of refractory bricks as in conventional kilns. For the entire glass liquid extrusion device, the temperature borne by the inner shell 12 and the support cylinder is relatively high, and they can be processed with corundum tubes, or partially with corundum tubes. The temperatures borne by other components have all dropped, and ordinary high-temperature resistant metal materials can meet the requirements. In this embodiment, they are all processed with high-temperature resistant stainless steel.
[0134] For the extrusion screw 30, the ventilation of the internal central axis hole 33 is beneficial to the cooling of the extrusion screw 30. Therefore, even if the screw portion 35 is in direct contact with the high-temperature glass liquid, under the cooling effect of the gas and the fact that the screw portion 35 itself is close to the outlet rather than in the center of the cavity 40, the screw portion 35 is made of high-temperature resistant stainless steel to meet the temperature resistance requirements.
[0135] Although the present invention is disclosed through the above embodiments, the scope of the present invention is not limited thereto, and the above components may be replaced with similar or equivalent elements known to those skilled in the art without departing from the concept of the present invention.
Claims
1. A glass liquid extrusion molding method, It is characterized in that It includes: conveying the molten glass to an extrusion device; The extrusion device is used to extrude the glass liquid from the annular discharge port.
2. The glass liquid extrusion molding method according to claim 1, It is characterized in that Before conveying the glass liquid to the extrusion device, the temperature of the glass liquid is adjusted to a first temperature, and the first temperature ranges from 900°C to 1200°C.
3. The glass liquid extrusion molding method according to claim 1, It is characterized in that When the glass liquid is extruded from the annular discharge port or after being extruded, gas is blown into the glass liquid extruded from the annular discharge port to expand the glass liquid, so that the glass liquid expands and becomes thinner.
4. The glass liquid extrusion molding method according to claim 3, It is characterized in that After the glass liquid is transported to the extrusion device, Driving the glass liquid to be transported along a first direction in the transport channel; The molten glass is squeezed into a mixing channel arranged circumferentially around the transmission channel, so that the molten glass passes through the mixing channel and is squeezed out from the annular discharge port.
5. The glass liquid extrusion molding method according to claim 4, It is characterized in that The mixing channel and the transmission channel are isolated and coaxial, and the mixing channel and the transmission channel are connected through a through hole arranged transversely to the first direction.
6. The glass liquid extrusion molding method according to claim 4, It is characterized in that A rotatable extrusion screw is provided in the transmission channel. The extrusion screw is arranged along a first direction. The glass liquid is driven to be transmitted along the first direction in the transmission channel by the extrusion screw.
7. The glass liquid extrusion molding method according to claim 6, It is characterized in that The discharge amount of the annular discharge port is adjusted by adjusting the rotation speed of the extrusion screw.
8. The glass liquid extrusion molding method according to claim 6, It is characterized in that The extrusion screw squeezes the molten glass in the transmission channel to drive the molten glass through the mixing channel and extrude it from the annular outlet.
9. The glass liquid extrusion molding method according to claim 4, It is characterized in that The glass liquid is extruded from the annular discharge port along a first direction; When gas is blown into the glass liquid extruded from the annular discharge port for expansion, gas is blown into the glass liquid along a first direction at a preset distance from the annular discharge port outside the transmission channel.