Red light emitting borosilicate perovskite quantum dot glass and preparation method thereof
By using autologous crystallization method in borosilicate perovskite quantum dot glass, combined with natural cooling and ball milling technology, red light-emitting borosilicate perovskite quantum dot glass was prepared, and annealing and The high energy consumption and environmental protection issues of heat treatment achieve an efficient and low-cost preparation process and improve the temperature resilience of the glass.
Patent Information
- Application Number
- CN202410973604.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The prior art requires annealing and heat treatment when preparing red light-emitting borosilicate perovskite quantum dot glass, resulting in high energy consumption, high cost, long process flow, unfavorable for environmental protection, and long-term stability cannot be guaranteed.
Perovskite quantum dot glass was obtained by mixing H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX and naturally cooled, and red light-emitting borosilicate perovskite quantum dot glass was prepared by ball milling, using autologous crystallization The method does not require annealing.
The preparation of red-light-emitting borosilicate perovskite quantum dot glass is realized, with excellent temperature resilience, simple method, energy-saving, and suitable for large-scale production.
Smart Images

Figure CN118908570A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solid luminescent materials, and in particular to a red light emitting borosilicate perovskite quantum dot glass and a preparation method thereof. Background Art
[0002] In recent years, all-inorganic perovskite quantum dots have attracted widespread attention due to their excellent optical properties such as high photoluminescence quantum yield, tunable luminescence in the entire visible light band, and high luminescence color purity, making them a strong candidate material for the manufacture of devices such as LEDs, liquid crystal displays, temperature sensors, and backlight displays. Traditional perovskite quantum dots are usually synthesized by chemical methods, but due to the ionic crystal characteristics and low formation energy of perovskite quantum dots, their long-term stability cannot be guaranteed, which seriously hinders their practical application in the optoelectronic field. Oxide glass materials have the advantages of high stability and easy preparation, so encapsulating perovskite quantum dots in inorganic glass materials has become an effective means to improve the stability of perovskite quantum dots.
[0003] Previously, most of the research work focused on green-light-emitting CsPbBr3 perovskite quantum dot glass, while there was relatively little research progress on red-light-emitting perovskite quantum dot glass. In addition, in the process of preparing CsPbBr3 perovskite quantum dot glass, annealing and heat treatment are often required, which not only increases energy consumption and costs, but also has a long process flow, slow production efficiency, and is not conducive to environmental protection.
[0004] Therefore, how to prepare red light emitting borosilicate perovskite quantum dot glass without annealing and heat treatment has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0005] The object of the present invention is to provide a red light emitting borosilicate perovskite quantum dot glass and a preparation method thereof. The preparation method provided by the present invention can make the borosilicate perovskite quantum dot glass have excellent temperature resilience without annealing and heat treatment.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing red light emitting borosilicate perovskite quantum dot glass, comprising the following steps:
[0008] (1) H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX are mixed and melted, and then naturally cooled to obtain perovskite quantum dot glass;
[0009] (2) ball-milling the perovskite quantum dot glass obtained in step (1) to obtain red light emitting borosilicate perovskite quantum dot glass.
[0010] Preferably, in step (1), the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX is (24-49): (9-34): (5-9): (13-17): 8: 19: 11.
[0011] Preferably, the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX is 39:19:7:15:8:19:11.
[0012] Preferably, in step (1), PbX2 is PbBr2 and / or PbI2.
[0013] Preferably, the PbX2 is PbBr2 and PbI2, and the molar ratio of PbBr2 and PbI2 is (6-8):(11-13).
[0014] Preferably, in step (1), NaX is NaBr and / or NaI.
[0015] Preferably, the NaX is NaBr and NaI, and the molar ratio of NaBr to NaI is (1-3):(8-10).
[0016] Preferably, in step (2), the rotation speed of the ball mill is 80 to 120 rpm, and the ball milling time is 1.5 to 3 hours.
[0017] Preferably, the ball milling speed is 100 rpm, and the ball milling time is 2 to 2.5 hours.
[0018] The present invention provides red light emitting borosilicate perovskite quantum dot glass prepared by the preparation method described in the above technical solution.
[0019] The present invention provides a method for preparing a red-light emitting borosilicate perovskite quantum dot glass, comprising the following steps: (1) mixing H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX, melting the mixture, and naturally cooling the mixture to obtain a perovskite quantum dot glass; (2) ball-milling the perovskite quantum dot glass obtained in step (1) to obtain a red-light emitting borosilicate perovskite quantum dot glass. The present invention obtains the red-light emitting borosilicate perovskite quantum dot glass by a self-crystallization method, and the preparation process does not require annealing and heat treatment. The method is simple and energy-saving, and can be mass-produced. The prepared red-light emitting borosilicate perovskite quantum dot glass has excellent temperature resilience. The results of the examples show that the red-light emitting borosilicate perovskite quantum dot glass provided by the present invention has excellent temperature resilience. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The XRD diagram of the red light emitting borosilicate perovskite quantum dot glass obtained in Examples 1 to 5;
[0021] Figure 2 TEM image of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 3;
[0022] Figure 3 This is a HTEM image of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 3;
[0023] Figure 4 is the emission spectrum of the red light emitting borosilicate perovskite quantum dot glass obtained in Examples 1 to 5;
[0024] Figure 5 This is a SEM image of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 2;
[0025] Figure 6 This is a magnified SEM image of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 2;
[0026] Figure 7 The temperature rise spectrum of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 3;
[0027] Figure 8 The cooling spectrum of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 3;
[0028] Fig. 9 This is a curve showing the change in luminescence intensity of the red light-emitting borosilicate perovskite quantum dot glass obtained in Example 3 during the heating and cooling processes. DETAILED DESCRIPTION
[0029] The present invention provides a method for preparing red light emitting borosilicate perovskite quantum dot glass, comprising the following steps:
[0030] (1) H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX are mixed and melted, and then naturally cooled to obtain perovskite quantum dot glass;
[0031] (2) ball-milling the perovskite quantum dot glass obtained in step (1) to obtain red light emitting borosilicate perovskite quantum dot glass.
[0032] The present invention mixes H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX, melts the mixture, and obtains perovskite quantum dot glass after natural cooling.
[0033] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or products prepared using processes well known to those skilled in the art.
[0034] In the present invention, the PbX2 is preferably PbBr2 and / or PbI2, more preferably PbBr2 and PbI2. In the present invention, when the PbX2 is PbBr2 and PbI2, the molar ratio of PbBr2 and PbI2 is preferably (6-8): (11-13), more preferably 7:12.
[0035] In the present invention, the NaX is preferably NaBr and / or NaI, more preferably NaBr and NaI. In the present invention, when the NaX is NaBr and NaI, the molar ratio of NaBr to NaI is preferably (1-3):(8-10), more preferably 2:9.
[0036] In the present invention, the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX is preferably (24-49): (9-34): (5-9): (13-17): 8: 19: 11, more preferably (34-44): (14-24): 7: 15: 8: 19: 11, and further preferably 39: 19: 7: 15: 8: 19: 11. The present invention can further improve the temperature resilience of the glass by controlling the amount relationship of the raw materials.
[0037] The present invention has no particular limitation on the specific operation of the mixing, which can be determined according to the technical common sense of those skilled in the art.
[0038] In the present invention, the melting is preferably carried out in a muffle furnace. The present invention has no particular limitation on the specific model of the muffle furnace, and a commercially available muffle furnace well known to those skilled in the art can be used.
[0039] In the present invention, the melting holding temperature is preferably 1050-1150°C, more preferably 1100°C; the melting holding time is preferably 5-40 minutes, more preferably 10-20 minutes. The present invention can ensure that the raw materials are completely melted to form a uniform glass melt by controlling the melting process parameters.
[0040] After melting, the present invention preferably pours the molten glass into a brass mold and then cools it naturally. The present invention can avoid a large increase in internal stress due to a too fast temperature drop through natural cooling.
[0041] After obtaining the perovskite quantum dot glass, the present invention ball-mills the perovskite quantum dot glass to obtain red light emitting borosilicate perovskite quantum dot glass.
[0042] In the present invention, the ball milling is preferably carried out in a ball mill. The present invention has no particular limitation on the specific model of the ball mill, and any ball mill well known to those skilled in the art can be used.
[0043] In the present invention, the rotation speed of the ball mill is preferably 80 to 120 rpm, more preferably 100 rpm; the time of the ball mill is preferably 1.5 to 3 hours, more preferably 2 to 2.5 hours. The present invention can improve the luminescence uniformity of the red light emitting borosilicate perovskite quantum dot glass by ball milling the glass, thereby improving the optical properties of the glass.
[0044] In the present invention, the particle size of the red light emitting borosilicate perovskite quantum dot glass is preferably 1 to 5 μm. The present invention can further improve the luminescence uniformity by controlling the particle size of the glass.
[0045] The present invention obtains red light emitting borosilicate perovskite quantum dot glass by a self-crystallization method. The preparation process does not require annealing and heat treatment. The method is simple and energy-saving and can be mass-produced. The prepared red light emitting borosilicate perovskite quantum dot glass has excellent temperature resilience.
[0046] The present invention provides a red light emitting borosilicate perovskite quantum dot glass prepared by the preparation method described in the above technical solution. The red light emitting borosilicate perovskite quantum dot glass prepared by the present invention has excellent temperature resilience.
[0047] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] Example 1
[0049] A method for preparing red light emitting borosilicate perovskite quantum dot glass, comprising the following steps:
[0050] (1) H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaBr and NaI are mixed and melted in a muffle furnace, and then poured into a brass mold and naturally cooled to room temperature to obtain perovskite quantum dot glass; the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaI and NaBr is 24:34:7:15:8:7:12:2:9; the melting holding temperature is 1100°C, and the melting holding time is 10 min;
[0051] (2) The perovskite quantum dot glass obtained in step (1) is ball-milled in a ball mill to obtain a red-light emitting borosilicate perovskite quantum dot glass with a particle size of 1 to 5 μm, which is denoted as PG1; the ball milling speed is 100 rpm and the ball milling time is 2 h.
[0052] Example 2
[0053] A method for preparing red light emitting borosilicate perovskite quantum dot glass, comprising the following steps:
[0054] (1) H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaBr and NaI are mixed and melted in a muffle furnace, and then poured into a brass mold and naturally cooled to room temperature to obtain perovskite quantum dot glass; the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaI and NaBr is 34:24:7:15:8:7:12:2:9; the melting holding temperature is 1100°C, and the melting holding time is 10 min;
[0055] (2) The perovskite quantum dot glass obtained in step (1) is ball-milled in a ball mill to obtain a red-light emitting borosilicate perovskite quantum dot glass with a particle size of 1 to 5 μm, which is denoted as PG2; the ball milling speed is 100 rpm and the ball milling time is 2 h.
[0056] Example 3
[0057] A method for preparing red light emitting borosilicate perovskite quantum dot glass, comprising the following steps:
[0058] (1) H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaBr and NaI are mixed and melted in a muffle furnace, and then poured into a brass mold and naturally cooled to room temperature to obtain perovskite quantum dot glass; the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaI and NaBr is 39:19:7:15:8:7:12:2:9; the melting holding temperature is 1100°C, and the melting holding time is 10 min;
[0059] (2) The perovskite quantum dot glass obtained in step (1) is ball-milled in a ball mill to obtain a red-light emitting borosilicate perovskite quantum dot glass with a particle size of 1 to 5 μm, which is denoted as PG3; the ball milling speed is 100 rpm and the ball milling time is 2 h.
[0060] Example 4
[0061] A method for preparing red light emitting borosilicate perovskite quantum dot glass, comprising the following steps:
[0062] (1) H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaBr and NaI are mixed and melted in a muffle furnace, and then poured into a brass mold and naturally cooled to room temperature to obtain perovskite quantum dot glass; the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaI and NaBr is 44:14:7:15:8:7:12:2:9; the melting holding temperature is 1100°C, and the melting holding time is 10 min;
[0063] (2) The perovskite quantum dot glass obtained in step (1) is ball-milled in a ball mill to obtain a red-light emitting borosilicate perovskite quantum dot glass with a particle size of 1 to 5 μm, which is denoted as PG4; the ball milling speed is 100 rpm and the ball milling time is 2 h.
[0064] Example 5
[0065] A method for preparing red light emitting borosilicate perovskite quantum dot glass, comprising the following steps:
[0066] (1) H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaBr and NaI are mixed and melted in a muffle furnace, and then poured into a brass mold and naturally cooled to room temperature to obtain perovskite quantum dot glass; the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbBr2, PbI2, NaI and NaBr is 49:9:7:15:8:7:12:2:9; the melting holding temperature is 1100°C, and the melting holding time is 10 min;
[0067] (2) The perovskite quantum dot glass obtained in step (1) is ball-milled in a ball mill to obtain a red-light emitting borosilicate perovskite quantum dot glass with a particle size of 1 to 5 μm, which is denoted as PG5; the ball milling speed is 100 rpm and the ball milling time is 2 h.
[0068] The red light emitting borosilicate perovskite quantum dot glasses obtained in Examples 1 to 5 were characterized by X-ray diffraction (XRD) (D2 phase shifter, Bruker, Karlsruhe). The results are shown in Figure 1 As shown. Figure 1 It can be seen that perovskite quantum dots are precipitated in the glass.
[0069] The red light emitting borosilicate perovskite quantum dot glass obtained in Example 3 was observed using a JEOL JEM-F200 transmission electron microscope (TEM). The obtained TEM image is shown in FIG. Figure 2 The obtained HTEM image is shown in Figure 3 As shown. Figures 2-3 It can be seen that many spherical particles are precipitated in the glass. The interplanar spacing of the particles is 0.29 nm, corresponding to the (200) crystal plane of CsPbBrI2 perovskite quantum dots, which further proves that CsPbBrI2 perovskite quantum dots have been successfully prepared in borosilicate glass by the self-crystallization method.
[0070] Figure 4 The emission spectra of the red light emitting borosilicate perovskite quantum dot glass obtained in Examples 1 to 5 are shown in FIG. Figure 4 It can be seen that the emission spectrum peak is located at 637-651nm. At the same time, the glass is brown under sunlight and emits bright red light under ultraviolet light.
[0071] The red light emitting borosilicate perovskite quantum dot glass obtained in Example 2 was observed using a scanning electron microscope, and the results obtained at different magnifications were as follows: Figure 5 and Figure 6 As shown. Figures 5-6 It can be seen that many holes are formed on the glass surface, and the large holes contain white substances. After analysis, it is found that the phase separation of borosilicate glass leads to holes on the glass surface. The white substance in the holes is the "nanoglass area", which is a mixture of perovskite quantum dots and glass. The perovskite quantum dots will precipitate from this substance. Phase separation is the reason for the self-crystallization of perovskite quantum dots.
[0072] Figure 7 is the heating spectrum of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 3, Figure 8 is the cooling spectrum of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 3, Fig. 9 This is the luminescence intensity variation curve of the red light emitting borosilicate perovskite quantum dot glass obtained in Example 3 during the heating and cooling process. Figures 7 to 9 It can be seen that when the temperature gradually rises from room temperature, the luminescence intensity of the CsPbBrI2 perovskite quantum dot glass gradually decreases, and when the temperature gradually drops to room temperature, the luminescence of the perovskite quantum dot glass gradually recovers, and at the same temperature, the intensity is even higher than when the temperature is increased, indicating that the borosilicate perovskite quantum dot glass obtained by the present invention has excellent temperature resilience.
[0073] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing red light emitting borosilicate perovskite quantum dot glass, comprising the following steps: (1) H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX are mixed and melted, and then naturally cooled to obtain perovskite quantum dot glass; (2) ball-milling the perovskite quantum dot glass obtained in step (1) to obtain red light emitting borosilicate perovskite quantum dot glass.
2. The preparation method according to claim 1, characterized in that: In the step (1), the molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX is (24-49): (9-34): (5-9): (13-17): 8: 19:
11.
3. The preparation method according to claim 2, characterized in that: The molar ratio of H3BO3, SiO2, ZnO, Na2CO3, Cs2CO3, PbX2 and NaX is 39:19:7:15:8:19:
11.
4. The preparation method according to claim 1, characterized in that: In the step (1), PbX2 is PbBr2 and / or PbI2.
5. The preparation method according to claim 4, characterized in that: The PbX2 is PbBr2 and PbI2, and the molar ratio of PbBr2 and PbI2 is (6-8):(11-13).
6. The preparation method according to claim 1, characterized in that: In the step (1), NaX is NaBr and / or NaI.
7. The preparation method according to claim 6, characterized in that: The NaX is NaBr and NaI, and the molar ratio of NaBr to NaI is (1-3):(8-10).
8. The preparation method according to claim 1, characterized in that: In the step (2), the rotation speed of the ball mill is 80 to 120 rpm, and the ball milling time is 1.5 to 3 hours.
9. The preparation method according to claim 8, characterized in that: The ball mill has a rotation speed of 100 rpm and a ball milling time of 2 to 2.5 hours.
10. Red light emitting borosilicate perovskite quantum dot glass prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
CsPbBr3 (cesium-lead-bromide) perovskite quantum dot fluorescent glass for display of wide color gamut and preparation method and application thereof
CN110294597A
Full-inorganic perovskite quantum dot fluorescent glass as well as preparation method and application thereof
CN113912291A
Perovskite quantum dot microcrystalline glass and preparation method thereof
CN114133141A
Al < 3 + >-doped CsPbBr3 quantum dot glass ceramic and preparation method thereof
CN114634312A
Full-inorganic perovskite quantum dot microcrystalline glass material and preparation method thereof
CN115124247A