Ultrathin flexible glass preparation method and ultrathin flexible glass
By adopting multi-stage difference high-performance glass preparation method in ultra-thin flexible glass, the problem of insufficient impact resistance in the bending area is solved through steps such as pattern design, etching and tempering, and achieving higher impact resistance and wider Application.
Patent Information
- Application Number
- CN202410921539.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
AI Technical Summary
The existing ultra-thin flexible glass has insufficient impact resistance in the bending zone, resulting in the problems of local stress concentration and poor impact performance during folding and use of the product.
Using the multi-stage difference high-performance glass preparation method, ultra-thin flexible glass with multi-layer structure is formed by preparing patterns, etching, thinning, stacking, cutting, machining, edge etching, tempering and surface etching on the glass substrate. , improve the impact resistance of the bending zone.
It improves the impact resistance of the bending and non-bending areas of ultra-thin flexible glass, enhances the overall impact resistance of the product, and enhances the application value of the product. It is suitable for folding screen electronic equipment and other electronic products.
Smart Images

Figure CN118908582A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ultra-thin flexible glass, and in particular, relates to a method for preparing ultra-thin flexible glass and the ultra-thin flexible glass. Background Art
[0002] With the rapid development of consumer electronic products, glass has been widely used in the electronics industry. The market has increasingly thinned the thickness of the protective glass for touch screen glass cover plates. Ultra-thin glass has become one of the important development trends of glass. Ultra-thin glass cover plates have attracted more and more attention from listed companies in the electronic display industry, and are mainly used in folding mobile phones, folding laptops and various wearable electronic devices. Ultra-thin flexible glass (UTG) refers to glass with a thickness of less than 100μm and is flexible. UTG is widely used in various electronic industries due to its high transparency, stability and impact resistance. Its easy-to-bend characteristics have marked a major milestone for the folding display industry, becoming an important player in the field of foldable flexible cover plates after CPI cover plates. With people's diversified demands for consumer products, UTG is designed to be thinner in order to ensure the bending performance and stability of the product, but such a design will lead to insufficient impact resistance of the product; therefore, a set of multi-segment high-performance glass products are designed according to different bending requirements; compared with the common flat UTG (ultra-thin flexible glass), the overall thickness of the middle part of the new ultra-thin flexible glass is thinner, which is used to reduce the local stress concentration when the flexible screen is folded, but there is a thickness difference in the middle part, which effectively improves the impact resistance of the bending area while ensuring bending.
[0003] The current thickness of ultra-thin glass is basically 30-100μm. UTG will lose some impact strength due to its thinner thickness. Conventional UFG (Ultra Flexible Glass) products with thick sides and thin middle have stress differences and expansion rate differences after strengthening. The product appearance is poor and not practical, and the thinner areas have the same poor impact performance problem as UTG.
[0004] It is hoped to provide an improved method for preparing ultra-thin flexible glass, particularly a method for improving product yield and enhancing the impact resistance of the product's bending zone. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing ultra-thin flexible glass, the purpose of which is to improve the impact resistance of the bending zone of the product.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is: a method for preparing ultra-thin flexible glass, comprising the steps of:
[0007] S1. preparing a pattern on a glass substrate;
[0008] S2, etching the glass substrate;
[0009] S3, thinning the glass substrate as a whole;
[0010] S4, stacking the glass substrates to form a main stack;
[0011] S5, cutting the main stack to obtain sub-stacks;
[0012] S6, machining the sub-stack;
[0013] S7, etching the edge of the sub-stack;
[0014] S8, performing tempering treatment;
[0015] S9, performing surface etching treatment;
[0016] S10: Cleaning.
[0017] In the step S1, an infrared laser is used to cut a pattern on the glass substrate.
[0018] In the step S3, the glass substrate is thinned by top spray thinning.
[0019] In the step S4, multiple glass substrates are bonded together by dispensing glue on the glass substrates, and the main stack is formed after the glue is cured.
[0020] In the step S5, the main stack is cut into target sizes using laser cutting to obtain a plurality of sub-stacks.
[0021] The step S6 comprises:
[0022] S601, CNC processing;
[0023] S602: Perform edge processing.
[0024] In the step S7, the edge of the sub-stack is treated by mixed acid.
[0025] In the step S8, the tempering treatment is performed for 17 to 20 minutes.
[0026] In the step S8, the temperature of the tempering treatment is 370-390°C.
[0027] The present invention also provides an ultra-thin flexible glass, which is manufactured using the ultra-thin flexible glass preparation method.
[0028] The method for preparing ultra-thin flexible glass of the present invention has a reasonable process route and a very high yield rate in the production process. The finished glass has high impact resistance, improves the impact strength of the product, and has mass production capability. It can effectively solve the problem of insufficient strength in the bending zone of conventional unequal thickness products in the current UTG and development process, and at the same time improves the strength of the non-bending zone of UTG. It has high application value and can be widely used in home appliance panels, smart phones, smart watches, tablet computers, wearable smart products, dashboards, etc., opening up a broad vision for folding screen electronic devices and providing a new possibility for the flexible screen market. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] This specification includes the following drawings, which show the following contents:
[0030] Figure 1 It is a flow chart of the method for preparing ultra-thin flexible glass of the present invention. DETAILED DESCRIPTION
[0031] The specific implementation methods of the present invention are further explained in detail below by describing the embodiments with reference to the accompanying drawings, with the aim of helping those skilled in the art to have a more complete, accurate and in-depth understanding of the concept and technical solution of the present invention and facilitating its implementation.
[0032] like Figure 1 As shown, the present invention provides a method for preparing ultra-thin flexible glass, comprising the following steps:
[0033] S1. preparing a pattern on a glass substrate;
[0034] S2, etching the glass substrate;
[0035] S3, thinning the glass substrate as a whole;
[0036] S4, stacking the glass substrates to form a main stack;
[0037] S5, cutting the main stack to obtain sub-stacks;
[0038] S6, machining the sub-stack;
[0039] S7, etching the edge of the sub-stack;
[0040] S8, performing tempering treatment;
[0041] S9, performing surface etching treatment;
[0042] S10: Cleaning.
[0043] Specifically, in the above step S1, an infrared laser is used to cut a preliminary pattern on the glass substrate (without cutting through), and the pattern includes but is not limited to stripe, dot and other patterns.
[0044] In the above step S2, a mixed acid solution of sulfuric acid, nitric acid, hydrofluoric acid, hydrochloric acid, etc. is used to etch and thin the glass substrate to form the final pattern in the bending area of the glass. If there are special requirements for the drawing, the design and processing can be carried out according to the drawing to improve the strength of the non-bending area of the product; this design can make the non-bending area thickness more than 100um; the bending area thickness can be as low as 30um; to ensure the uniformity of the plate thickness after thinning.
[0045] In the above step S3, the glass substrate is thinned by top spraying. First, the glass substrate is fixed in a vertical clamping manner, and then the top spraying treatment is performed. The thinning acid etching amount of the glass substrate is about 200-400um. Because the acid etching rate of the upper and lower parts of the product is inconsistent during the thinning process, multiple chamfering treatments are performed during the process to improve the uniformity of the product thickness. The main principle of thinning is that hydrofluoric acid reacts with silicon dioxide on the glass surface to generate fluorosilicic acid to achieve the effect of glass thinning.
[0046] In the above step S4, multiple glass substrates are bonded together by dispensing glue on the glass substrates. After the glue is cured, a main stack is formed, which is convenient for subsequent edge processing. Moreover, after the glue is cured, the flexible product can be effectively protected.
[0047] In the above step S4, glue dispensing is performed by a continuous glue dispensing machine or a coating glue dispensing machine.
[0048] In the above step S5, the edges of all glass substrates constituting the main stack are aligned, and the main stack is cut into target sizes using laser cutting to obtain a plurality of sub-stacks.
[0049] In the above step S5, laser cutting uses fully automatic infrared picosecond cutting, which can accurately and effectively cut the product into the target size, facilitating subsequent processing; because the laser cannot process curved corners (there is a high risk of splintering and fragmentation).
[0050] The above step S6 includes:
[0051] S601, CNC processing;
[0052] S602: Perform edge processing.
[0053] In the above step S601, CNC processes the product through a numerically controlled machine tool to make the product reach a desired shape.
[0054] In the above step S602, edge processing is mainly performed by physically polishing the edges of the sub-stack. Physical polishing mainly involves edge polishing of the ultra-thin flexible glass by an edge polishing machine to ensure that the edges of the glass are smooth and free of burrs; at the same time, the product dimensional accuracy is improved.
[0055] In the above step S7, the edge of the sub-stack is processed by mixed acid. The edge etching is mainly to process the edge of the product by mixed acid, so that the edge of the product has a certain strength and has the possibility of bending.
[0056] In the above step S8, the sub-stack is first debonded and sliced to obtain multiple pieces of glass, and then the glass is chemically tempered. Chemical tempering is mainly a process of sodium-potassium ion exchange under high temperature conditions, using the squeezing effect generated by the volume difference between the two to improve the surface strength and flexibility of the glass. The tempering time is 17 to 20 minutes, and the temperature of the tempering is 370 to 390°C.
[0057] In the above step S9, the surface etching is mainly to perform micro-etching treatment on the surface of the tempered glass, and the main purpose is to repair the defects generated during the manufacturing process and the defects magnified after tempering.
[0058] In the above step S10, the glass is finally cleaned by ultrasonic cleaning and then dried to obtain the final ultra-thin flexible glass.
[0059] The above-mentioned flexible ultra-thin glass preparation method is easy to operate, has a wide processing range, a short processing cycle, can realize mass production planning, the glass edge and surface are processed accordingly, the yield is high, and the processed finished glass has an impact resistance similar to that of conventional cover plates, which can meet the current market demand for cover plates of foldable electronic products and has good use value.
[0060] The present invention also provides an ultra-thin flexible glass, which is manufactured using the ultra-thin flexible glass preparation method.
[0061] The ultra-thin flexible glass includes a bending zone and a non-bending zone. The bending zone is located in the middle of the ultra-thin flexible glass, and the non-bending zone is located on both sides of the bending zone. A strip pattern is set in the bending zone, which can reduce the local stress concentration when the flexible screen is folded while ensuring bending, thereby improving the impact resistance of the product. No pattern is set in the non-bending zone. The non-patterned zone increases the thickness of the non-bending zone of the product through multiple step differences, improves the performance of the non-bending zone of the product, and makes the performance of the non-bending zone reach the thickness and strength similar to that of a conventional cover plate. The bending zone of the multi-step high-performance flexible glass is designed with a pattern thinned according to the bending requirements or designed with a pattern after overall thinning, to reduce the local stress concentration when the flexible screen is folded; while ensuring bending, the impact resistance of the bending area is effectively improved.
[0062] This ultra-thin flexible glass can not only enhance the novelty of the appearance of smart terminal products, but also bring excellent touch feel. At the same time, it meets the design requirements of 3C products and is widely used in various 3C product designs, such as folding smartphones, folding tablet computers, wearable smart products, dashboards, etc., and is favored by consumers.
[0063] Embodiment 1
[0064] This embodiment provides a method for preparing ultra-thin flexible glass, comprising the following steps:
[0065] S1. preparing a pattern on a glass substrate;
[0066] S2, etching the glass substrate;
[0067] S3, thinning the glass substrate as a whole;
[0068] S4, stacking the glass substrates to form a main stack;
[0069] S5, cutting the main stack to obtain sub-stacks;
[0070] S6, machining the sub-stack;
[0071] S7, etching the edge of the sub-stack;
[0072] S8, performing tempering treatment;
[0073] S9, performing surface etching treatment;
[0074] S10: Cleaning.
[0075] In this embodiment, the glass substrate is AS87 raw glass produced by Schott.
[0076] In the above step S1, an infrared laser is used to cut a pattern on the glass substrate (without cutting through), and the pattern includes but is not limited to stripe, dot and other patterns.
[0077] In the above step S2, a mixed acid solution such as sulfuric acid, nitric acid, hydrofluoric acid, hydrochloric acid, etc. is used to etch and thin the glass substrate.
[0078] In the above step S3, the glass substrate is thinned by top spray thinning.
[0079] In the above step S4, the plurality of glass substrates are bonded together by a resin adhesive strip, and the resin adhesive strip is cured to form a main stacked body.
[0080] In the above step S5, the edges of all glass substrates constituting the main stack are aligned, and the main stack is cut into target sizes using laser cutting to obtain a plurality of sub-stacks.
[0081] In the above step S6, the target size is ground by a CNC machine tool, and then edge processing is performed to physically polish the edge of the sub-stack, so that the edge of the product is in a relatively excellent state.
[0082] In the above step S7, the edge of the sub-stack is treated with mixed acid to further strengthen the edge of the product; the C value of the product edge is 5-25μm; and the edge collapse is less than 20μm; liquid seepage is not allowed (edge abnormality caused by degumming during edge strengthening).
[0083] In the above step S8, after the sub-stack is debonded and sliced, a plurality of sheets of glass are obtained, and then the glass is chemically toughened.
[0084] In the above step S8, when chemical tempering is performed, the temperature is 380°C, the solution used is molten potassium nitrate, the purity of the molten potassium nitrate is 99.9%, and the tempering duration is 18 minutes. After tempering, the CS (surface compressive stress) of the glass can reach 730±50MPa, and the DOL (depth of stress layer) can reach 9±2μm.
[0085] In the above step S9, surface etching is mainly for micro-etching the surface of tempered glass, the main purpose of which is to repair the defects generated during the process and the defects magnified after tempering. After etching, the CS of the glass is 650±50MPa, and the DOL is 8±2μm; after testing, the Assy of the glass pattern area is 100-130mm, and the Assy of the glass non-pattern area is 150-200mm; dynamic bending 30W+ radius R0.8-R3 can be achieved; the Assy of the ultra-thin glass with an analog thickness of 30μm is greatly improved after tempering at 380℃ for 12min; the bending R3 of the ultra-thin glass with an analog thickness of 100μm is greatly improved after tempering at 380℃ for 20min; and there is no obvious difference in appearance from ultra-thin and thick glass; at the same time, it has both the bending ability of thin products and the impact resistance of thick products.
[0086] In the above step S10, the glass is finally cleaned by ultrasonic cleaning and then dried to obtain the final ultra-thin flexible glass.
[0087] In this embodiment, the thickness of the ultra-thin flexible glass in the bending zone is 30-50 μm, and the thickness of the non-bending zone is 100 μm.
[0088] The present invention is described above by way of example in conjunction with the accompanying drawings. Obviously, the specific implementation of the present invention is not limited to the above-mentioned methods. As long as various non-substantial improvements are made using the method concept and technical solution of the present invention; or the above concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for preparing ultra-thin flexible glass, characterized in that: Includes steps: S1. Preparing a pattern on a glass substrate; S2, etching the glass substrate; S3, thinning the glass substrate as a whole; S4, stacking the glass substrates to form a main stack; S5, cutting the main stack to obtain sub-stacks; S6, machining the sub-stack; S7, etching the edge of the sub-stack; S8, performing tempering treatment; S9, performing surface etching treatment; S10: Cleaning.
2. The method for preparing ultra-thin flexible glass according to claim 1, characterized in that: In the step S1, an infrared laser is used to cut a pattern on the glass substrate.
3. The method for preparing ultra-thin flexible glass according to claim 1, characterized in that: In the step S3, the glass substrate is thinned by top spray thinning.
4. The method for preparing ultra-thin flexible glass according to any one of claims 1 to 3, characterized in that: In the step S4, multiple glass substrates are bonded together by dispensing glue on the glass substrates, and the main stack is formed after the glue is cured.
5. The method for preparing ultra-thin flexible glass according to any one of claims 1 to 3, characterized in that: In the step S5, the main stack is cut into target sizes using laser cutting to obtain a plurality of sub-stacks.
6. The method for preparing ultra-thin flexible glass according to any one of claims 1 to 3, characterized in that: The step S6 comprises: S601, CNC processing; S602: Perform edge processing.
7. The method for preparing ultra-thin flexible glass according to any one of claims 1 to 3, characterized in that: In the step S7, the edge of the sub-stack is treated by mixed acid.
8. The method for preparing ultra-thin flexible glass according to any one of claims 1 to 3, characterized in that: In the step S8, the tempering treatment is performed for 17 to 20 minutes.
9. The method for preparing ultra-thin flexible glass according to any one of claims 1 to 3, characterized in that: In the step S8, the temperature of the tempering treatment is 370-390°C.
10. Ultra-thin flexible glass, characterized in that: The ultra-thin flexible glass is manufactured using the ultra-thin flexible glass preparation method described in any one of claims 1 to 9.