Special glass coating device and coating process thereof

Through laser deposition and ion implantation technology, the problem of high heat input in special glass coating technology is solved, uniform deposition and high-quality film are achieved, reducing the risk of substrate deformation, and improving the optical and chemical properties of the film.

CN118908587AInactive Publication Date: 2024-11-08徐州市威固特种玻璃有限公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410952973.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing special glass coating technology is relatively high in terms of heat input, increasing the thermal impact of the glass substrate and increasing the risk of substrate deformation and cracks.

Method used

Using laser deposition technology, metal targets are uniformly deposited on the glass surface through scanning with the center of the circle expanding outward. Combined with ion implantation technology, the chemical composition and structure of the film are adjusted, the heat input is reduced, and the deposition uniformity is ensured through real-time monitoring and microscopy analysis. and quality.

Benefits of technology

It reduces the thermal impact of the glass substrate, reduces the risk of deformation and cracks, realizes the deposition of high-purity materials, improves the optical performance and chemical stability of the film, and reduces environmental pollution and waste liquid treatment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908587A_ABST
    Figure CN118908587A_ABST
Patent Text Reader

Abstract

The invention discloses a special glass coating device and a coating process thereof, and relates to the technical field of glass coating. The problems of substrate deformation and cracks caused by high heat input of a traditional coating method are solved. The method specifically comprises the following steps that a metal material meeting the requirement is selected and cut into blocks meeting the target material size requirement, and the cut metal target material is subjected to surface impurity removal, polishing and grinding treatment for standby application; a laser beam is focused on the metal target material to evaporate the metal target material to generate plasma, and then the plasma is deposited on the surface of the special glass; gradually depositing a metal target material on the surface of the special glass through laser deposition to form a required film structure; and the coated special glass is subjected to annealing treatment in a heat treatment process, and the chemical components and the structure of the film are changed by injecting ions into the surface of the film. In the laser deposition process, the heat input is low, the heat influence on the special glass substrate is reduced, and the risks of deformation and cracks of the substrate are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of glass coating, and in particular to a special glass coating device and a coating process thereof. Background Art

[0002] Special glass coating is a technology that coats special materials on the surface of glass to change the optical, electrical, and thermal properties of the glass, as well as to enhance its corrosion resistance. This technology is usually used to manufacture glass products with specific functions, such as solar glass, anti-glare glass, heat-insulating glass, etc. Special glass coating technology is widely used in various fields such as architecture, automobiles, aerospace, electronics, optics, etc. By coating different materials on the surface of glass, special functions such as anti-glare, heat insulation, UV protection, bulletproof, and explosion-proof can be achieved.

[0003] Special glass coating technology can improve the optical properties of glass, such as light transmittance, reflectivity, and transmissivity; it can also improve the thermal properties of glass, such as heat insulation and thermal insulation; it can also enhance the corrosion resistance of glass and extend its service life. Special glass coating technology can effectively reduce the energy consumption of buildings and cars and improve indoor comfort. For example, thermal insulation coating can reduce the air conditioning load in summer and reduce energy consumption; anti-ultraviolet coating can protect indoor furniture and floors from fading due to ultraviolet rays.

[0004] After searching, the Chinese patent application number CN2012101137549 discloses a blue glass coating method including the following steps: measuring the transmittance of the blue glass to light of different wavelengths: constructing a spectral curve of the blue glass according to the transmittance of the different wavelengths; selecting a film system according to the spectral curve; coating the blue glass according to the film system. Measure the transmittance of light of different wavelengths relative to the blue glass, construct a curve based on the measured transmittance, and the curve is the inherent spectral curve of the blue glass; select a film system according to the spectral curve of the blue glass, and then coat the blue glass according to the film system. The film system selected according to the spectral curve of the blue glass can meet the transmittance requirements of light of different wavelengths. The blue glass coating method in the above patent has the following shortcomings:

[0005] Although the above coating method can control the transmittance of light of different wavelengths relative to the coated blue glass to meet the different light transmittance requirements of light of different wavelengths relative to the coated blue glass, the above coating method has relatively high heat input, which increases the thermal impact on the glass substrate and increases the risk of deformation and cracks of the substrate. Summary of the invention

[0006] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a special glass coating device and a coating process thereof.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A special glass coating process comprises the following steps:

[0009] S1: Material preparation: Select metal materials that meet the requirements, cut them into blocks that meet the target size requirements, and perform surface impurity removal, polishing and grinding on the cut metal targets for use;

[0010] S2: Laser deposition: focusing the laser beam onto the metal target, causing it to evaporate, generate plasma, and then deposit on the specialty glass surface;

[0011] S3: Thin film formation: Through laser deposition, the metal target is gradually deposited on the surface of the special glass to form the required thin film structure;

[0012] S4: Post-treatment: The coated special glass is placed in a heat treatment for annealing, and ions are implanted into the film surface to change the chemical composition and structure of the film.

[0013] Preferably, the specific steps of the laser deposition are:

[0014] S21: Adjust the laser power, wavelength and pulse width according to the characteristics of the metal target and deposition requirements;

[0015] S22: The laser emits a laser beam to scan the metal target through the reflector, and the metal target is focused and evaporated by the laser beam to generate plasma;

[0016] S23: The metal target material evaporated by the focused laser beam and generated plasma diffuses to the surroundings and deposits on the surface of the special glass.

[0017] The scanning method with the center of the circle expanding outward can ensure that the laser deposition is evenly distributed on the entire surface, thereby improving the uniformity of the coating and covering a larger surface range, so that the laser deposition can be completed more quickly, improving production efficiency. At the same time, the scanning radius and speed can be adjusted as needed to achieve flexible control of the deposition shape and size. It is suitable for special glass surfaces of various shapes and sizes and meets the processing needs of different special glasses.

[0018] Furthermore: the power of the laser is 6-35W, the wavelength is 400-1100nm, and the pulse width is 7-48ns.

[0019] On the basis of the above scheme: the scanning speed of the laser is 8-15mm / s, the scanning method is to expand outward from the center of the circle, the supply speed of the metal target is 2.1-3.2cm / s, and the curvature radius of the reflector is 6mm-14mm.

[0020] A better solution among the above solutions is: real-time monitoring of step S3, the specific steps of which are:

[0021] S31: Real-time monitoring of film deposition by monitoring the reflectivity change of the laser beam on the film surface;

[0022] S32: Real-time observation and imaging of thin films using optical microscopy to evaluate the surface morphology, structure, and uniformity of the films;

[0023] S33: Real-time analysis of the surface morphology of the film using scanning electron microscopy to evaluate the flatness, roughness, and structural features of the film.

[0024] As a further solution of the present invention: the reflectivity of the film surface in step S31 can be calculated by the following formula:

[0025]

[0026] Wherein, R is the reflectivity of the film, N1 is the refractive index of air or vacuum, N2 is the refractive index of the metal target, θ1 is the incident angle of light, and θ2 is the refraction angle of light.

[0027] When the film begins to deposit, the reflectivity will gradually increase. When the film reaches a certain thickness, the reflectivity tends to stabilize. In this way, the deposition rate, uniformity and quality of the film can be understood in real time through the data calculation of the film surface reflectivity. In addition, the abnormal data of the film surface reflectivity can be used to deduce that there are problems with the film deposition and adjust the deposition parameters in time.

[0028] Meanwhile, in the step S4, ions are implanted into the surface of the film to change the chemical composition and structure of the film. The specific steps are as follows:

[0029] S41: placing the coated special glass into a vacuum chamber;

[0030] S42: An ion source is introduced into a vacuum chamber, and the ions are accelerated to a high speed through an accelerator, and then injected into the film through an electric field control. The chemical composition and structure of the film surface are changed by ion injection, thereby enhancing its surface properties such as hardness, wear resistance, and corrosion resistance. At the same time, the adhesion between the film and the special glass is improved, the bonding force of the film is enhanced, and its service life and stability are improved. A solid protective layer can be formed on the surface of the film, thereby improving the scratch resistance and durability of the film, and improving the transparency, reflectivity and optical properties of the special glass.

[0031] As a preferred embodiment of the present invention, the ion source uses any one of nitrogen ions, oxygen ions and argon ions, the voltage of the accelerator is 3-10KV, the electric field strength of the accelerator is 230-860V / cm, and the ion injection time is 12-35min.

[0032] A coating device for a special glass coating process includes a laser for laser deposition, a reflector for focusing the laser beam, a metal target for making a thin film, an optical microscope for thin film imaging, a scanning electron microscope for analyzing the surface morphology of the thin film, a vacuum chamber for ion implantation, an ion source for emitting ions, and an accelerator for controlling ions.

[0033] The beneficial effects of the present invention are:

[0034] 1. A special glass coating device and coating process thereof. During the laser deposition process of the special glass, the heat input is low, which can reduce the thermal impact on the special glass substrate and reduce the risk of substrate deformation and cracks. It does not require the use of chemical solutions and a large amount of chemicals, which reduces the impact on the environment and the cost of waste liquid treatment. At the same time, it achieves the deposition of high-purity materials, and the film quality is more stable with better optical properties and chemical stability.

[0035] 2. A special glass coating device and coating process thereof, a scanning method with the center of the circle expanding outward can ensure that the laser deposition is evenly distributed on the entire surface, thereby improving the uniformity of the coating, and can cover a larger surface range, so that the laser deposition can be completed more quickly, improving production efficiency. At the same time, the scanning radius and speed can be adjusted as needed, thereby achieving flexible control of the deposition shape and size, and is suitable for special glass surfaces of various shapes and sizes to meet the processing requirements of different special glasses.

[0036] 3. A special glass coating device and its coating process. When the film begins to be deposited, the reflectivity will gradually increase. When the film reaches a certain thickness, the reflectivity tends to be stable. In this way, the deposition rate, uniformity and quality of the film can be understood in real time through the data calculation of the film surface reflectivity. In addition, the abnormal data of the film surface reflectivity can be used to deduce the problems of the film deposition and adjust the deposition parameters in time.

[0037] 4. This special glass coating device and its coating process change the chemical composition and structure of the film by ion implantation into the film surface, thereby enhancing its surface properties such as hardness, wear resistance, and corrosion resistance, while improving the adhesion between the film and the special glass, enhancing the bonding force of the film, and improving its service life and stability. It can also form a solid protective layer on the film surface, improve the scratch resistance and durability of the film, and improve the transparency, reflectivity, and optical properties of the special glass.

[0038] 5. This special glass coating device and its coating process can understand the composition distribution, grain structure, grain boundary and grain size of the film by observing the cross-section or surface morphology of the film; in the special glass coating process, uniformity is crucial to the optical and functional properties of the film. Through real-time observation and imaging, defects, impurities or uneven thickness on the surface of the film can be found, and the process parameters can be adjusted in time to ensure the uniformity of the film.

[0039] 6. A special glass coating device and its coating process. The scanning electron microscope has the advantages of high resolution and depth information, making it an ideal tool for studying the surface morphology of thin films. The scanning electron microscope provides high-resolution images of the surface and can clearly observe the microstructure of the film surface, including surface roughness, particle size and distribution. This helps to evaluate the roughness of the film and provides an important reference for the optical and functional properties of the film. It can also provide information on the structural characteristics of the film, including grain size, grain boundary distribution, crystal structure, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A schematic diagram of a process flow of a special glass coating process proposed by the present invention;

[0041] Figure 2 A schematic diagram of the process of laser deposition in a special glass coating process proposed by the present invention;

[0042] Figure 3 A schematic diagram of a process for monitoring the surface of a thin film in a special glass coating process proposed by the present invention;

[0043] Figure 4 The present invention provides a schematic diagram of the process of injecting ions into the surface of a thin film in a special glass coating process. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0045] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0046] A special glass coating process, such as Figure 1 As shown, the following steps are included:

[0047] S1: Material preparation: Select metal materials that meet the requirements, cut them into blocks that meet the target size requirements, and perform surface impurity removal, polishing and grinding on the cut metal targets for use; the metal material is any one of aluminum, silver, nickel and chromium;

[0048] S2: Laser deposition: focusing the laser beam onto the metal target to evaporate it, generate plasma, and then deposit it on the surface of the special glass; the laser beam uses any one of argon ion laser, argon neon laser and carbon dioxide laser;

[0049] S3: Thin film formation: Through laser deposition, the metal target is gradually deposited on the surface of the special glass to form the required thin film structure;

[0050] S4: Post-treatment: The coated special glass is placed in a heat treatment for annealing, and ions are implanted into the film surface to change the chemical composition and structure of the film.

[0051] To ensure uniform deposition of thin films, Figure 2 As shown; the specific steps of the laser deposition are:

[0052] S21: According to the characteristics of the metal target and the deposition requirements, the laser power is adjusted to 6-35W, the laser wavelength is 400-1100nm, and the laser pulse width is 7-48ns; ensuring the appropriate intensity and focusing of the laser beam;

[0053] S22: The laser emits a laser beam to scan the metal target through the reflector, the scanning speed is 8-15 mm / s, the scanning method is a method of expanding outward from the center of the circle, the supply speed of the metal target is 2.1-3.2 cm / s, wherein the curvature radius of the reflector is 6 mm-14 mm, and the metal target is focused by the laser beam to evaporate and generate plasma;

[0054] S23: The metal target material evaporated by the focused laser beam and generated plasma diffuses to the surroundings and deposits on the surface of the special glass.

[0055] The scanning method with the center of the circle expanding outward can ensure that the laser deposition is evenly distributed on the entire surface, thereby improving the uniformity of the coating and covering a larger surface range, so that the laser deposition can be completed more quickly, improving production efficiency. At the same time, the scanning radius and speed can be adjusted as needed to achieve flexible control of the deposition shape and size. It is suitable for special glass surfaces of various shapes and sizes and meets the processing needs of different special glasses.

[0056] In order to ensure the film thickness, uniformity and quality, such as Figure 3 As shown; the S3 step is monitored in real time, and its specific steps are:

[0057] S31: Monitor the deposition of thin films in real time by monitoring the reflectivity change of the laser beam on the film surface; by monitoring the reflectivity change of the laser beam, the thickness information of the film can be obtained in real time. This method has high sensitivity and real-time performance, can accurately monitor the deposition of thin films, help adjust the deposition rate and terminate the deposition process.

[0058] S32: Use an optical microscope to observe and image the film in real time to evaluate the surface morphology, structure and uniformity of the film; by observing the cross-section or surface morphology of the film, you can understand the composition distribution, grain structure, grain boundaries and grain size of the film; in the special glass coating process, uniformity is crucial to the optical and functional properties of the film. Through real-time observation and imaging, you can find defects, impurities or uneven thickness on the surface of the film, and adjust the process parameters in time to ensure the uniformity of the film.

[0059] S33: Real-time analysis of the surface morphology of the film using scanning electron microscopy to evaluate the flatness, roughness, and structural features of the film.

[0060] Scanning electron microscopy has the advantages of high resolution and depth information, making it an ideal tool for studying the surface morphology of thin films. Scanning electron microscopy can provide high-resolution images of the surface and clearly observe the microstructure of the film surface, including surface roughness, particle size and distribution. This helps to evaluate the roughness of the film and provides an important reference for the optical and functional properties of the film. It can also provide information on the structural characteristics of the film, including grain size, grain boundary distribution, crystal structure, etc.

[0061] These structural features have an important influence on the mechanical, optical and chemical properties of the film. The flatness, roughness and structural characteristics of the film can be comprehensively evaluated, providing important information for optimizing the film preparation process and improving the film quality and performance.

[0062] The reflectivity of the film surface in step S31 can be calculated by the following formula:

[0063]

[0064] Wherein, R is the reflectivity of the film, N1 is the refractive index of air or vacuum, N2 is the refractive index of the metal target, θ1 is the incident angle of light, and θ2 is the refraction angle of light; when the film begins to deposit, the reflectivity will gradually increase, and when the film reaches a certain thickness, the reflectivity tends to be stable. In this way, the deposition rate, uniformity and quality of the film can be understood in real time through the data calculation of the film surface reflectivity, and the abnormal data of the film surface reflectivity can be used to deduce the problems of the film deposition and adjust the deposition parameters in time;

[0065] like Figure 4 As shown, in the step S4, ions are implanted into the film surface to change the chemical composition and structure of the film. The specific steps are as follows:

[0066] S41: Place the coated special glass into a vacuum chamber; processing in a vacuum chamber can prevent the external environment from contaminating or oxidizing the film surface, maintain the purity of the film, and help improve the performance and characteristics of the film to meet specific application requirements.

[0067] S42: An ion source is introduced into the vacuum chamber, the ions are accelerated to a high speed by an accelerator, and the ions are injected into the film by electric field control; through electric field control and accelerator, it can be ensured that the ions are injected into the film at a high speed, thereby achieving precise control and improvement of the surface properties of the material.

[0068] The ion source uses any one of nitrogen ions, oxygen ions and argon ions, and the voltage of the accelerator is 3-10KV, the electric field strength of the accelerator is 230-860V / cm, and the ion injection time is 12-35min;

[0069] Ion implantation changes the chemical composition and structure of the film surface, thereby enhancing its surface properties such as hardness, wear resistance, and corrosion resistance. At the same time, it improves the adhesion between the film and special glass, enhances the bonding force of the film, and improves its service life and stability. It can also form a solid protective layer on the film surface, improve the film's scratch resistance and durability, and improve the transparency, reflectivity, and optical properties of special glass.

[0070] Different from traditional processes, the heat input of special glass during laser deposition is lower, which can reduce the thermal impact on the special glass substrate and the risk of substrate deformation and cracks. It does not require the use of chemical solutions and large amounts of chemicals, thus reducing the impact on the environment and the cost of waste liquid treatment. At the same time, it achieves the deposition of high-purity materials, and the film quality is more stable with better optical properties and chemical stability.

[0071] A special glass coating device includes a laser for laser deposition used in the above coating process, a reflector for focusing the laser beam, a metal target for making a thin film, an optical microscope for thin film imaging, a scanning electron microscope for analyzing the surface morphology of the thin film, a vacuum chamber for ion implantation, an ion source for emitting ions, and an accelerator for controlling ions.

[0072] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A special glass coating process, characterized in that: The following steps are involved: S1: Material preparation: Select metal materials that meet the requirements, cut them into blocks that meet the target size requirements, and perform surface impurity removal, polishing and grinding on the cut metal targets for use; S2: Laser deposition: focusing the laser beam onto the metal target, causing it to evaporate, generate plasma, and then deposit on the specialty glass surface; S3: Thin film formation: Through laser deposition, the metal target is gradually deposited on the surface of the special glass to form the required thin film structure; S4: Post-treatment: The coated special glass is placed in a heat treatment for annealing, and ions are implanted into the film surface to change the chemical composition and structure of the film.

2. A special glass coating process according to claim 1, characterized in that: The specific steps of the laser deposition are: S21: Adjust the laser power, wavelength and pulse width according to the characteristics of the metal target and deposition requirements; S22: The laser emits a laser beam to scan the metal target through the reflector, and the metal target is focused and evaporated by the laser beam to generate plasma; S23: The metal target material evaporated by the focused laser beam and generated plasma diffuses to the surroundings and deposits on the surface of the special glass.

3. A special glass coating process according to claim 2, characterized in that: The power of the laser is 6-35W, the wavelength is 400-1100nm, and the pulse width is 7-48ns.

4. A special glass coating process according to claim 2, characterized in that: The scanning speed of the laser is 8-15 mm / s, the scanning mode is a mode of expanding from the center of the circle outward, the supply speed of the metal target is 2.1-3.2 cm / s, and the curvature radius of the reflector is 6 mm-14 mm.

5. A special glass coating process according to claim 1, characterized in that: The S3 step is monitored in real time, and its specific steps are as follows: S31: Real-time monitoring of film deposition by monitoring the reflectivity change of the laser beam on the film surface; S32: Real-time observation and imaging of thin films using optical microscopy to evaluate the surface morphology, structure, and uniformity of the films; S33: Real-time analysis of the surface morphology of the film using scanning electron microscopy to evaluate the flatness, roughness, and structural features of the film.

6. A special glass coating process according to claim 5, characterized in that: The reflectivity of the film surface in step S31 can be calculated by the following formula: Wherein, R is the reflectivity of the film, N1 is the refractive index of air or vacuum, N2 is the refractive index of the metal target, θ1 is the incident angle of light, and θ2 is the refraction angle of light.

7. A special glass coating process according to claim 1, characterized in that: In the step S4, ions are implanted into the surface of the film to change the chemical composition and structure of the film. The specific steps are as follows: S41: placing the coated special glass into a vacuum chamber; S42: An ion source is introduced into the vacuum chamber, the ions are accelerated to a high speed by an accelerator, and the ions are injected into the film by controlling the electric field.

8. A special glass coating device and coating process according to claim 7, characterized in that: The ion source uses any one of nitrogen ions, oxygen ions and argon ions, and the voltage of the accelerator is 3-10KV, the electric field strength of the accelerator is 230-860V / cm, and the time of ion injection is 12-35min.

9. A coating device for the special glass coating process according to any one of claims 1 to 8, characterized in that: It includes the laser used for laser deposition, the reflector for focusing the laser beam, the metal target for making thin films, the optical microscope for thin film imaging, the scanning electron microscope for analyzing the surface morphology of the thin film, the vacuum chamber for ion implantation, the ion source for emitting ions, and the accelerator for controlling ions.

Citation Information