Heat treatment method based on cold spraying of Al-Mg composite coating
Through cold spraying technology and low-temperature heat treatment, the Al-Mg composite coating has been solved for the density reduction and cracking problems at high temperatures, and its corrosion resistance and service life in complex environments are improved.
Patent Information
- Application Number
- CN202410934480.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-29
AI Technical Summary
The Al-Mg composite coating becomes loose after a long period of high-temperature heat treatment, and the density decreases. Cracking or peeling is easily generated between the coating and the substrate, affecting its corrosion resistance and service life.
The Al-Mg composite coating was sprayed on the pretreated substrate by cold spraying, and the diffusion annealing heat treatment was carried out at 250°C for 6 to 8 hours. After removal, it was cooled to room temperature to prepare a coating with a density.
It improves the density and corrosion resistance of the coating, enhances its protective effect in complex environments, extends its service life, and does not adversely affect the performance of the substrate.
Smart Images

Figure CN119040869A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material anticorrosion, and in particular relates to a heat treatment method based on cold spraying Al-Mg composite coating. Background Art
[0002] Steel is still the most commonly used structural material at this stage, and corrosion is one of the main reasons for the failure of steel. For the structural materials of marine equipment that are in the harsh environment of the marine atmosphere for a long time, the importance of corrosion protection is particularly important. There are many means of steel protection, and the most widely used is metal protective coating. Cold spraying is a new type of spraying technology that uses high-pressure gas to carry powder particles into the spray gun from the axial direction to generate supersonic airflow. After the powder particles are accelerated by the airflow, they hit the surface of the substrate in a completely solid state, produce large plastic deformation and deposit on the surface of the substrate to form a coating. The temperature during the cold spraying process is low, and it has the characteristics of solid deposition at low temperature. Vacuum heat treatment is often used to improve the coating structure, thereby improving its corrosion resistance and mechanical properties. However, due to the different properties and deformation degrees of different materials, the most suitable heat treatment temperature for different materials is also different.
[0003] Due to its abundant reserves and obvious passivation effect, Al has become one of the preferred materials for metal protective coatings. However, the passivation film of Al coating in seawater will be destroyed by Cl- and eventually develop into pitting. In order to improve the anodic performance of Al, elements such as Zn and Mg are often added. Mg can react with oxygen and water in the environment to form stable oxides and hydroxides. This reaction provides additional protection for the substrate and further enhances the protective effect of the coating. When the coating is scratched or locally damaged, Mg can quickly react with oxygen and water in the environment to form a protective layer. This feature helps to repair the damaged area and prevent further corrosion, thereby improving the self-healing ability of the coating. Adding an appropriate amount of Mg can also improve the mechanical properties of the composite material. Therefore, adding a small amount of Mg can not only improve the sacrificial ability of the coating, but also reduce the accumulation of corrosion products to form a harder shell-like protective layer, greatly improving the corrosion resistance and service life of the coating. However, long-term high-temperature heat treatment will make the Al-Mg composite coating loose and reduce its density, and cracks are easily generated between the coating and the substrate, and even the coating will peel off.
[0004] Therefore, preparing Al-Mg composite coating and performing low-temperature heat treatment to obtain a protective coating with good density and high corrosion resistance is an important idea to solve the problem of steel corrosion. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a heat treatment method based on cold sprayed Al-Mg composite coating.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a heat treatment method based on cold sprayed Al-Mg composite coating, comprising:
[0009] Using spherical Al powder and Mg powder as raw materials, Al-Mg composite coating was sprayed on the pretreated substrate by cold spraying process;
[0010] The Al-Mg composite coating is packaged in vacuum, subjected to diffusion annealing heat treatment at 250° C. for 6 to 8 hours, taken out and air-cooled to room temperature to obtain a heat-treated coating.
[0011] As a preferred solution of the heat treatment method of the present invention, wherein: in terms of element mass percentage, the Al is 91-99wt.%, and the Mg is 1-9wt.%.
[0012] As a preferred solution of the heat treatment method of the present invention, wherein: in terms of element mass percentage, the Al is 99wt.%, and the Mg is 1wt.%.
[0013] As a preferred solution of the heat treatment method of the present invention, wherein: in terms of element mass percentage, the Al is 95wt.%, and the Mg is 5wt.%.
[0014] As a preferred solution of the heat treatment method of the present invention, wherein: in terms of element mass percentage, the Al is 91wt.%, and the Mg is 9wt.%.
[0015] As a preferred embodiment of the heat treatment method of the present invention, the cold spraying process includes:
[0016] The powder feeding gas and working gas are compressed air, the spraying angle is 90°, the gas pressure is 0.99MPa, the gas heating temperature is 400℃, and the powder feeding amount is 50g / min;
[0017] During cold spraying, the distance between the spray gun and the substrate surface is 12 mm, and the relative movement speed between the spray gun and the substrate is 5 to 8 mm / s.
[0018] As a preferred embodiment of the heat treatment method of the present invention, the preparation method of the pre-treated substrate includes:
[0019] The substrate was pretreated and grease was removed by ultrasonic cleaning with acetone;
[0020] Use white corundum for sandblasting to remove rust and increase the surface roughness of the substrate.
[0021] As a preferred solution of the heat treatment method of the present invention, the substrate comprises Q235 steel.
[0022] Another object of the present invention is to overcome the deficiencies in the prior art and provide an Al-Mg composite coating prepared by a heat treatment method.
[0023] Another object of the present invention is to overcome the deficiencies in the prior art and provide an Al-Mg composite coating for use in long-term corrosion protection of steel in various complex environments such as the atmosphere and the ocean.
[0024] Beneficial effects of the present invention:
[0025] (1) The cold spraying technology used in the present invention has low working temperature when preparing the coating. The temperature during the cold spraying process is relatively low, and it has the characteristics of solid deposition at low temperature, small thermal effect on the substrate, no oxidation, grain growth, phase change occurs during the spraying process, and low residual tensile stress.
[0026] (2) The present invention adopts a cold spraying process to prepare the target coating, which is simple in process; adding Al2O3 ceramic phase powder to the powder can reduce the porosity of the coating and increase the density of the tissue.
[0027] (3) The addition of an appropriate amount of Mg element in the present invention further enhances the protective effect of the coating, improves the self-healing ability of the coating and improves the mechanical properties of the composite material.
[0028] (4) In the present invention, heat treatment of the coating at the selected annealing temperature can enhance the coating performance without affecting the performance of the body itself. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0030] Figure 1 This is a cross-sectional scanning electron microscope image of the Al-1Mg coating prepared in Example 1 of the present invention.
[0031] Figure 2 This is a cross-sectional scanning electron microscope image of the Al-5Mg coating prepared in Example 2 of the present invention.
[0032] Figure 3 This is a cross-sectional scanning electron microscope image of the Al-9Mg coating prepared in Example 3 of the present invention.
[0033] Figure 4 This is a cross-sectional scanning electron microscope image of the Al-1Mg coating prepared in Comparative Example 1 of the present invention.
[0034] Figure 5 This is a cross-sectional scanning electron microscope image of the Al-5Mg coating prepared in Comparative Example 2 of the present invention.
[0035] Figure 6 This is a cross-sectional scanning electron microscope image of the Al-9Mg coating prepared in Comparative Example 3 of the present invention.
[0036] Figure 7 The electrochemical test results of the Al-Mg composite coatings in the embodiments of the present invention and the comparative examples after being immersed in a 3.5% NaCl solution for 480 hours.
[0037] Figure 8 The hardness test results of the Al-Mg composite coatings in the embodiments of the present invention and the comparative examples are shown. DETAILED DESCRIPTION
[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0039] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0040] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments. The raw materials in the present invention are all common commercially available products.
[0041] Example 1
[0042] (1) Build an XY automation platform and check the operation of the spray robot to see if there is any shaking or jamming;
[0043] (2) Pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0044] (3) Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0045] (4) Spherical Al powder and Mg powder are used as raw materials, with a weight ratio of Al 99wt.%, Mg 1wt.%, and then mixed thoroughly and placed in a vacuum drying oven for 2 hours.
[0046] (5) The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.99 MPa, the powder feeding temperature is 400°C, the powder feeding amount is 50 g / min, the distance between the spray gun and the substrate is 12 mm, and the spray gun moving speed is 5-8 mm / s. These parameters are used to prepare the cold spray composite coating;
[0047] (6) After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Mg composite coating is obtained.
[0048] (7) The sample was packaged in vacuum and subjected to diffusion annealing heat treatment at 250°C for 8 hours, and then taken out and air-cooled to room temperature.
[0049] (8) Use a solder gun to solder the wires and seal with resin to expose only the test surface.
[0050] (9) The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0051] (10) Two batches of samples were encapsulated using hot mounting powder, and only the exposed test surface was subjected to a neutral salt spray test using 5% NaCl solution;
[0052] Hardness test was performed using a microhardness tester.
[0053] The scanning electron microscope image of the cross section of the heat-treated cold-sprayed Al-Mg composite coating obtained in Example 1 (7) is as follows: Figure 1 As shown, the scanning electron microscopy results show that after a long period of low-temperature heat treatment, the coating becomes dense, and the Mg element and Al element in the coating fully react to form a large amount of Al3Mg2 phase.
[0054] Example 2
[0055] (1) Build an XY automation platform and check the operation of the spray robot to see if there is any shaking or jamming;
[0056] (2) Pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0057] (3) Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0058] (4) Use spherical Al powder and Mg powder as raw materials, with a weight ratio of Al 95wt.%, Mg 5wt.%, and mix well, then put into a vacuum drying oven and dry for 2 hours.
[0059] (5) The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.99 MPa, the powder feeding temperature is 400°C, the powder feeding amount is 50 g / min, the distance between the spray gun and the substrate is 12 mm, and the spray gun moving speed is 5-8 mm / s. These parameters are used to prepare the cold spray composite coating;
[0060] (6) After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Mg composite coating is obtained.
[0061] (7) The sample was packaged in vacuum, and subjected to diffusion annealing heat treatment at 250°C for 8 hours, and then taken out and air-cooled to room temperature.
[0062] (8) Use a solder gun to solder the wires and seal with resin to expose only the test surface.
[0063] (9) The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0064] (10) Two batches of samples were encapsulated using hot mounting powder, and only the exposed test surface was subjected to a neutral salt spray test using 5% NaCl solution;
[0065] Hardness test was performed using a microhardness tester.
[0066] The scanning electron microscope image of the cross section of the heat-treated cold-sprayed Al-Mg composite coating obtained in Example 2 (7) is as follows: Figure 2 As shown, the scanning electron microscopy results show that after a long period of low-temperature heat treatment, compared with Example 1, it can be seen that as the Mg content increases, the Al3Mg2 in the coating increases and the coating becomes denser.
[0067] Example 3
[0068] (1) Build an XY automation platform and check the operation of the spray robot to see if there is any shaking or jamming;
[0069] (2) Pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0070] (3) Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0071] (4) Use spherical Al powder and Mg powder as raw materials, with a weight ratio of Al 91wt.%, Mg 9wt.%, and mix well, then put into a vacuum drying oven and dry for 2 hours.
[0072] (5) The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.99 MPa, the powder feeding temperature is 400°C, the powder feeding amount is 50 g / min, the distance between the spray gun and the substrate is 12 mm, and the spray gun moving speed is 5-8 mm / s. These parameters are used to prepare the cold spray composite coating;
[0073] (6) After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Mg composite coating is obtained.
[0074] (7) The sample was packaged in vacuum and subjected to diffusion annealing heat treatment at 250°C for 8 hours, and then taken out and air-cooled to room temperature.
[0075] (8) Use a solder gun to solder the wires and seal with resin to expose only the test surface.
[0076] (9) The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0077] (10) Two batches of samples were encapsulated using hot mounting powder, and only the exposed test surface was subjected to a neutral salt spray test using 5% NaCl solution;
[0078] Hardness test was performed using a microhardness tester.
[0079] The scanning electron microscope image of the cross section of the heat-treated cold-sprayed Al-Mg composite coating obtained in Example 3 (7) is as follows: Figure 3 As shown, the scanning electron microscopy results show that after a long period of low-temperature heat treatment, although it can be seen that compared with Examples 1 and 2, as the Mg content increases, the Al3Mg2 in the coating increases, but the excess Mg also causes some holes in the coating.
[0080] Comparative Example 1
[0081] (1) Build an XY automation platform and check the operation of the spray robot to see if there is any shaking or jamming;
[0082] (2) Pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0083] (3) Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0084] (4) Spherical Al powder and Mg powder are used as raw materials, with a weight ratio of Al 99wt.%, Mg 1wt.%, and then mixed thoroughly and placed in a vacuum drying oven for 2 hours.
[0085] (5) The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.99 MPa, the powder feeding temperature is 400°C, the powder feeding amount is 50 g / min, the distance between the spray gun and the substrate is 12 mm, and the spray gun moving speed is 5-8 mm / s. These parameters are used to prepare the cold spray composite coating;
[0086] (6) After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Mg composite coating is obtained.
[0087] (7) The sample was packaged in vacuum and subjected to diffusion annealing heat treatment at 500°C for 8 hours, and then taken out and air-cooled to room temperature.
[0088] (8) Use a solder gun to solder the wires and seal with resin to expose only the test surface.
[0089] (9) The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0090] (10) Two batches of samples were encapsulated with hot mounting powder, and only the exposed test surface was subjected to a neutral salt spray test using a 5% NaCl solution. A microhardness tester was used to perform a hardness test.
[0091] The scanning electron microscope image of the cross section of the heat-treated cold-sprayed Al-Mg composite coating obtained in (7) of Comparative Example 1 is as follows: Figure 4 As shown, the scanning electron microscopy results show that after a long period of high-temperature heat treatment, the coating becomes loose, and there are obvious cracks between the coating and the substrate, and Fe2Al5 phase is formed at the connection between the coating and the substrate.
[0092] Comparative Example 2
[0093] (1) Build an XY automation platform and check the operation of the spray robot to see if there is any shaking or jamming;
[0094] (2) Pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0095] (3) Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0096] (4) Use spherical Al powder and Mg powder as raw materials, with a weight ratio of Al 95wt.%, Mg 5wt.%, and mix well, then put into a vacuum drying oven and dry for 2 hours.
[0097] (5) The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.99 MPa, the powder feeding temperature is 400°C, the powder feeding amount is 50 g / min, the distance between the spray gun and the substrate is 12 mm, and the spray gun moving speed is 5-8 mm / s. These parameters are used to prepare the cold spray composite coating;
[0098] (6) After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Mg composite coating is obtained.
[0099] (7) The sample was packaged in vacuum and subjected to diffusion annealing heat treatment at 500°C for 8 hours, and then taken out and air-cooled to room temperature.
[0100] (8) Use a solder gun to solder the wires and seal with resin to expose only the test surface.
[0101] (9) The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0102] (10) Two batches of samples were encapsulated with hot mounting powder, and only the exposed test surface was subjected to a neutral salt spray test using a 5% NaCl solution. A microhardness tester was used to perform a hardness test.
[0103] The scanning electron microscope image of the cross section of the heat-treated cold-sprayed Al-Mg composite coating obtained in (7) of Comparative Example 2 is as follows: Figure 5 As shown, the scanning electron microscopy results show that after a long period of high-temperature heat treatment, the coating becomes loose and there are obvious cracks between the coating and the substrate, but the density is better than that of comparative example 1, and Fe2Al5 phase is also formed at the connection between the coating and the substrate.
[0104] Comparative Example 3
[0105] (1) Build an XY automation platform and check the operation of the spray robot to see if there is any shaking or jamming;
[0106] (2) Pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0107] (3) Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0108] (4) Use spherical Al powder and Mg powder as raw materials, with a weight ratio of Al 91wt.%, Mg 9wt.%, and mix well, then put into a vacuum drying oven and dry for 2 hours.
[0109] (5) The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.99 MPa, the powder feeding temperature is 400°C, the powder feeding amount is 50 g / min, the distance between the spray gun and the substrate is 12 mm, and the spray gun moving speed is 5-8 mm / s. These parameters are used to prepare the cold spray composite coating;
[0110] (6) After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Mg composite coating is obtained.
[0111] (7) The sample was packaged in vacuum and subjected to diffusion annealing heat treatment at 500°C for 8 hours, and then taken out and air-cooled to room temperature.
[0112] (8) Use a solder gun to solder the wires and seal with resin to expose only the test surface.
[0113] (9) The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0114] (10) Two batches of samples were encapsulated with hot mounting powder, and only the exposed test surface was subjected to a neutral salt spray test using a 5% NaCl solution. A microhardness tester was used to perform a hardness test.
[0115] The scanning electron microscope image of the cross section of the heat-treated cold-sprayed Al-Mg composite coating obtained in (7) of Comparative Example 3 is as follows: Figure 6 As shown, the scanning electron microscopy results show that the coating with excessive Mg addition has peeled off after a long period of high temperature heat treatment.
[0116] Performance Test:
[0117] Relevant performance tests were performed on the embodiments of the present invention and the comparative examples, and the test results are shown below.
[0118] (1) Vickers hardness test: the test standard is GB / T 4340.1-2024. Take one hot-mounted sample in step (10) of the embodiment and the comparative example respectively, and use 400 mesh, 1000 mesh and 2000 mesh sandpaper to grind the coating surface of the sample to be tested, so that the sample surface is smooth and scratch-free;
[0119] Then use the microhardness tester to test the hardness, select five points to calculate the average value, the results are shown in Table 1 and Figure 8 shown.
[0120] Table 1
[0121]
[0122] Conclusion: The hardness of the cold-sprayed Al-Mg composite coating at different heat treatment temperatures shows a trend of first increasing and then decreasing with the increase of Mg content, and it can be seen that the hardness of the coating under low-temperature annealing is higher than that under high-temperature annealing. The hardness is highest when the annealing temperature is 250℃ and the Mg content is 5wt.%.
[0123] (2) Neutral salt spray test: The test standard is GB / T 10125-2021. The hot-mounted samples in step (10) of the embodiment and the comparative example are cleaned with anhydrous ethanol and blown dry. The sample weight is weighed using an electronic balance. A 5 wt.% NaCl solution is prepared and added to a salt spray chamber. The sample is placed in the salt spray chamber for testing.
[0124] The temperature of the salt spray box was maintained at 35±1°C, pH=6.5-7.2, and the corrosion time was 480 hours. The results are shown in Table 2.
[0125] Table 2
[0126]
[0127] In this study, the weight gain method was used to measure the corrosion rate of the sample, and the calculation formula is:
[0128] V=(W2-W1)·S -1 ·T -1
[0129] Where, V: corrosion rate of galvanized sheet, unit: g·m -2 ·h -1
[0130] W1: weight of the sample before corrosion, g
[0131] W2: weight of the sample after corrosion, g
[0132] S: Sample exposure area, m 2
[0133] T: corrosion cycle, h
[0134] Conclusion: The corrosion rate of cold-sprayed Al-Mg composite coatings at different heat treatment temperatures increases first and then decreases with the increase of Mg content, and it can be seen that the corrosion rate of samples treated at low temperature is lower than that treated at high temperature.
[0135] When the annealing temperature is 250℃ and the Mg content is 5wt.%, the salt spray corrosion rate of the coating is 0.6813g / (m 2 .h), at which point the corrosion rate is the lowest.
[0136] (3) Electrochemical test: The test standard is GBT40299-2021. The samples soaked in step (9) of the embodiment and the comparative example were subjected to electrochemical impedance test and potentiodynamic polarization curve test. The results are shown in Table 3 and Figure 7 shown.
[0137] Table 3
[0138]
[0139]
[0140] Conclusion: Among the embodiments and comparative examples, the coating prepared in Example 2 has the highest self-corrosion potential and the lowest self-corrosion current density, so it has the smallest corrosion tendency, the slowest corrosion rate and the best corrosion resistance.
[0141] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A heat treatment method based on cold sprayed Al-Mg composite coating, characterized in that: include, Using spherical Al powder and Mg powder as raw materials, Al-Mg composite coating was sprayed on the pretreated substrate by cold spraying process; The Al-Mg composite coating is packaged in vacuum, subjected to diffusion annealing heat treatment at 250° C. for 6 to 8 hours, taken out and air-cooled to room temperature to obtain a heat-treated coating.
2. The heat treatment method according to claim 1, characterized in that: In terms of element mass percentage, the Al is 91-99 wt.%, and the Mg is 1-9 wt.%.
3. The heat treatment method according to claim 2, characterized in that: In terms of element mass percentage, the Al is 99 wt.%, and the Mg is 1 wt.%.
4. The heat treatment method according to claim 2, characterized in that: Calculated by element mass percentage, the Al is 95 wt.%, and the Mg is 5 wt.%.
5. The heat treatment method according to claim 2, characterized in that: In terms of element mass percentage, the Al is 91 wt.%, and the Mg is 9 wt.%.
6. The heat treatment method according to any one of claims 1 to 5, characterized in that: The cold spraying process comprises: The powder feeding gas and working gas are compressed air, the spraying angle is 90°, the gas pressure is 0.99MPa, the gas heating temperature is 400℃, and the powder feeding amount is 50g / min; During cold spraying, the distance between the spray gun and the substrate surface is 12 mm, and the relative movement speed between the spray gun and the substrate is 5 to 8 mm / s.
7. The heat treatment method according to claim 6, characterized in that: The preparation method of the pretreated substrate comprises: The substrate was pretreated and grease was removed by ultrasonic cleaning with acetone; Use white corundum for sandblasting to remove rust and increase the surface roughness of the substrate.
8. The heat treatment method according to claim 7, characterized in that: The substrate comprises steel Q235.
9. An Al-Mg composite coating obtained by the heat treatment method according to any one of claims 1 to 8.
10. Application of the Al-Mg composite coating as claimed in claim 9 in long-term corrosion protection of steel in various complex environments such as atmosphere and ocean.
Citation Information
Patent Citations
Preparation method for cold spraying of aluminum-based composite wear-resistant coating on surface of magnesium alloy