Cementing material as well as preparation method and application thereof

By using the gelling materials based on steel metallurgy solid waste, the hydration reaction is stimulated and regulated by composite excitants to form a high-performance C-H-S gel and calcium vanadium stone structure, the poor backfill effect and environmental pollution of mine filling gelling materials are solved, and the problem of poor backfill effect and environmental pollution of mine filling gelling materials is achieved. Efficient and low-cost mine filling effect.

CN118908600APending Publication Date: 2024-11-08GUANGDONG HUAXIN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411026919.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing mine filling gelling materials have problems such as poor backfill effect, high production costs, and easy to lead to environmental pollution. In particular, cement materials have poor consolidation performance, ease of water loss, and serious heavy metal pollution in fine-grained filling, which limits their large amounts. Scale application.

Method used

Using gelling materials based on steel metallurgical solid waste, the hydration reaction is stimulated and regulated through specific group distribution ratios and composite excitants to form a dense microstructure in which C-H-S gel and calcium vanadium stone develop synergistically, and improve the compressive strength of gelling materials and Resistant properties.

Benefits of technology

It has achieved low-cost and efficient mine filling gelling materials, with compressive strength reaching 2 to 3 times that of cement, better impermeability and reduced leaching concentration of heavy metal ions, suitable for large-scale applications and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968805060000071
    Figure BDA0004968805060000071
  • Figure BDA0004968805060000081
    Figure BDA0004968805060000081
  • Figure BDA0004968805060000082
    Figure BDA0004968805060000082
Patent Text Reader

Abstract

The invention discloses a cementing material as well as a preparation method and application thereof, and relates to the technical field of cementing materials. The cementing material is prepared from the following components in parts by mass: 10 to 30 parts of steel slag, 5 to 30 parts of roasting dedusting ash, 3 to 10 parts of desulfurized fly ash, 30 to 50 parts of slag and 5 to 10 parts of exciting agent. The gelling material can replace a traditional gelling material, a backfill body formed by the gelling material has high compressive strength and high anti-permeability performance, the compressive strength can reach 2-3 times that of cement under the condition of the same cement-sand ratio, the anti-permeability pressure is higher, namely, the anti-permeability performance is better, meanwhile, the leaching concentration of heavy metal ions is lower, the gelling material is more environmentally friendly, and the backfill body is suitable for large-scale popularization and application. The production cost can be reduced, the requirement of large-scale production can be met, and the method is suitable for filling materials and is applied to mine backfilling, especially backfilling of fine-fraction multi-metal tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gelling materials, and in particular to a gelling material and a preparation method and application thereof. Background Art

[0002] At present, the cementitious materials used for mine filling mainly include cement, high-water materials, alkali-activated cementitious materials or paste filling materials.

[0003] Among them, cement as a cementitious material has two major problems: first, it has poor consolidation performance for fine-grained materials such as tailings and sand and materials with high mud content, and the filling body consumes a large amount of material to reach the designed strength; second, cement slurry is easy to separate and bleed, and cement loss is serious. High-water material is a cementitious material prepared by the process of producing cement using bauxite, gypsum, limestone, etc. as the main raw materials. It also has the problems of easy water loss and weathering, long-term stability cannot be guaranteed, production ingredients need to be specially prepared and fired, quality requirements and costs are high, and improper slurry ratio and mixing control are prone to non-setting phenomenon. These shortcomings limit the large-scale application of high-water materials in mine filling. The shortage of bauxite resources required for high-water materials and the easy loss of control of the matching operation of the two slurries also restrict the development of this filling material. Alkali-activated cementitious materials refer to a type of cementitious materials formed by the reaction of materials with volcanic ash activity or potential hydraulic hardness with alkaline activators. At present, alkali-activated cementitious materials have the following problems: first, there are many factors affecting the performance of alkali-activated cementitious materials, which lacks systematicity; second, the difference in the composition of different industrial wastes has a great impact on the performance fluctuation of alkali-activated cementitious materials; third, there is a lack of water-reducing agents. Water-reducing agents that have a good water-reducing effect on silicate cement are usually ineffective on alkali-activated materials. Therefore, the current application of alkali-activated cementitious materials is also subject to great restrictions.

[0004] Paste filling material is a paste with enough fine particles, which can make the viscosity of the flow field greater than the inertial force and reach a saturated structured flow slurry. Filling mines with paste filling materials has the advantages of maintaining the stability of surrounding rocks, reducing surface subsidence, improving the recovery rate of natural resources and protecting the environment. It can completely solve the environmental pollution problem of tailings ponds and ensure the sustainable development of mines. However, because paste filling technology uses ordinary cement as a gelling material, it must use higher-power delivery pumps and stirring devices, and efficient and stable concentration devices, which brings about problems such as large equipment investment, complex management and operation, and high cement material costs. The treatment technology of overflow tailings is also not mature enough, and it is usually abandoned in tailings ponds, causing environmental pollution and occupying limited land resources.

[0005] It can be seen that the current mine filling materials have poor backfilling effects, such as water seepage problems, high production costs, environmental pollution such as heavy metal pollution, and difficulty in large-scale application. Therefore, according to the requirements of mining production, it is necessary to develop a mine filling cementitious material with good professional characteristics, wide source of raw materials, low price and good backfilling effect. Summary of the invention

[0006] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the purpose of the present invention is to provide a cementitious material that effectively utilizes steel metallurgical solid waste, activates the activity based on the steel mill metallurgical solid waste, and has the characteristics of low cost, good backfill effect and high anti-seepage performance.

[0007] A second aspect of the present invention provides a method for preparing a gelling material.

[0008] A third aspect of the present invention provides a filling material.

[0009] A fourth aspect of the present invention provides a use of a gelling material or a filling material.

[0010] In order to achieve the above object, the technical solution adopted by the present invention is:

[0011] The first aspect of the present invention provides a gelling material, which comprises the following components by weight:

[0012] 10-30 parts of steel slag, 5-30 parts of roasting dust ash, 3-10 parts of desulfurization ash, 30-50 parts of slag, and 5-10 parts of activator.

[0013] The present invention is based on steel slag, slag, roasting dust ash, desulfurization ash and other components, and uses an activator to stimulate and control the hydration reaction schedule, continuously and fully stimulate the hydration reaction activity of solid waste particles, so that the gelled slurry forms a dense microstructure morphology of CHS gel and calcium vanadium synergistic development, and obtains a high-performance gelled material. Due to the different solid waste production processes and reaction conditions, their chemical compositions and mineral structures are quite different, and their gelling activities are also different. For example, steel slag has low early activity, while mineral powder has good comprehensive activity. Therefore, the present invention maximizes the gelling activity of different components as much as possible through a specific component ratio, and improves the various performance indicators of the gelled material after gelling.

[0014] Among them, slag is the waste slag discharged from iron smelting and is rapidly cooled by water quenching, and steel slag is the slag discharged from steelmaking and is heated once. These smelting waste slags have certain gelling activity, which is beneficial to improving the performance of cementitious materials, and they belong to general industrial solid waste. Using them to develop cementitious materials can realize the reuse of metallurgical solid waste.

[0015] The roasted dust ash mainly contains CaO, which has water retention and plasticity in the cementitious material. In the hydration reaction, it can provide OH through the following reactions: - :CaO+H2O=Ca(OH)2.

[0016] Desulfurized ash contains more CaSO3·0.5H2O, CaCO3, Ca(OH)2, and also contains a small amount of unreacted desulfurizer CaO and a trace amount of mullite, which can provide an appropriate amount of CaO and sulfate in the hydration reaction. In the process of forming the filling body by the cementitious material of the present invention, the roasted dust removal ash can provide an alkaline environment to ensure the later strength growth, and the desulfurized ash provides sulfate ions in the alkaline environment to ensure the early strength growth, thereby improving the comprehensive strength of the filling body formed by the cementitious material.

[0017] In some embodiments of the present invention, the metallurgical solid waste used in the cementitious material is Shaogang metallurgical solid waste, including Shaogang steel slag, Shaogang desulfurization ash, Shaogang roasting dust ash, and Shaogang slag.

[0018] In some embodiments of the present invention, the steel slag is steel slag powder; the slag is slag powder.

[0019] In some embodiments of the present invention, the specific surface area of ​​the steel slag powder and the slag powder is 350-450m 2 / kg.

[0020] In some embodiments of the present invention, the molar ratio of calcium to silicon in the steel slag is (2-4):1.

[0021] In some embodiments of the present invention, the molar ratio of calcium to silicon in the steel slag is (2-3):1.

[0022] In some specific embodiments of the present invention, the molar ratio of calcium to silicon in the steel slag is (2.5-3):1.

[0023] In some embodiments of the present invention, the molar ratio of silicon to aluminum in the steel slag is (0.2-0.6):1.

[0024] In some embodiments of the present invention, the molar ratio of silicon to aluminum in the steel slag is (0.3-0.5):1.

[0025] In some specific embodiments of the present invention, the molar ratio of silicon to aluminum in the steel slag is (0.4-0.5):1.

[0026] In some examples of the present invention, the molar ratio of silicon to aluminum in the steel slag is (0.4-0.45):1.

[0027] In some embodiments of the present invention, the molar ratio of calcium to silicon in the slag is (1-3):1.

[0028] In some embodiments of the present invention, the molar ratio of calcium to silicon in the slag is (1-2):1.

[0029] In some specific embodiments of the present invention, the molar ratio of calcium to silicon in the slag is (1-1.5):1.

[0030] In some embodiments of the present invention, the molar ratio of silicon to aluminum in the slag is (0.7-1):1.

[0031] In some embodiments of the present invention, the molar ratio of silicon to aluminum in the slag is (0.8-0.9):1.

[0032] In some specific embodiments of the present invention, the molar ratio of silicon to aluminum in the slag is (0.85-0.9):1.

[0033] In some embodiments of the present invention, the glass content in the steel slag is 80-95%.

[0034] In some embodiments of the present invention, the content of glass in the steel slag is 85-90%.

[0035] In some embodiments of the present invention, the glass content in the slag is 85-95%.

[0036] In some embodiments of the present invention, the glass content in the slag is 90-95%.

[0037] In some embodiments of the present invention, the steel slag includes the following components by mass fraction: 4-5% aluminum oxide, 35-40% calcium oxide, and 13-14% silicon oxide.

[0038] In some embodiments of the present invention, the slag includes the following components by mass fraction: 14-15% aluminum oxide, 40-42% calcium oxide, and 30-35% silicon oxide.

[0039] The gelling activity of solid waste from the steel industry is the basis for the development of cementitious materials. The present invention further limits the calcium-silicon molar ratio (Ca / Si), aluminum-silicon molar ratio (Al / Si) and glass content, especially the aluminum-silicon molar ratio, to regulate the reaction of mineral powder when synthesizing new materials, and further improve the compressive strength and impermeability of cementitious materials. It should be noted that the glass content and the content of components such as alumina are calculated separately, and there is no relationship that the sum is equal to 100%.

[0040] In some embodiments of the present invention, the roasted dust ash includes the following components by mass fraction: 67-69% calcium oxide, 7-9% silicon oxide, 2-4% magnesium oxide, 1-2% aluminum oxide, and 19-21% calcium carbonate.

[0041] In some embodiments of the present invention, the desulfurization ash includes the following main chemical components by mass fraction: 0.1-0.2% aluminum oxide, 51-52% calcium oxide, 0.5-0.6% iron oxide, 0.3-0.4% potassium oxide, 0.7-0.8% magnesium oxide, 0.05-0.06% sodium oxide, 1.2-1.3% silicon oxide, 14-15% sulfur trioxide, 0.009-0.010% phosphorus pentoxide, 0-0.0001% thallium oxide, and 1.6-1.7% chlorine.

[0042] Steel slag, mineral slag, dust removal ash and desulfurization ash also contain other trace components.

[0043] In some embodiments of the present invention, the activator is a composite activator; the composite activator includes a silicate activator and an alkaline activator.

[0044] At present, the activation of solid wastes such as slag, steel slag, desulfurization ash, and tailings generally adopts a single chemical activation route such as alkali, sulfate, and chloride. For complex solid waste materials with dense crystals and large grains such as steel slag, their activation ability is relatively poor, and it is difficult to solve the industry problem of early strength, early setting, and continuous growth of late strength of cementitious slurry. The present invention further adopts a composite activation method combining multiple activation methods, using silicate activators and alkaline solid activators, wherein the silicate activator can meet the early strength requirements, and the alkaline activator ensures the late strength growth, further solving the technical problem of continuous growth of cementitious material strength.

[0045] In some embodiments of the present invention, the mass ratio of the silicate activator to the alkaline activator is (8-10):1.

[0046] The second aspect of the present invention provides a method for preparing the gelling material according to the first aspect of the present invention, comprising the following steps:

[0047] The cementitious material is obtained by mixing steel slag, roasting dust removal ash, desulfurization ash, slag and activator in proportion.

[0048] The third aspect of the present invention provides a filling material, comprising aggregate and cementitious material; the cementitious material is the cementitious material described in the first aspect of the present invention.

[0049] In some embodiments of the present invention, the mass ratio of the cementitious material to the aggregate is 1:(4-12).

[0050] The third aspect of the present invention provides a use of the cementitious material described in the first aspect of the present invention or the filling material described in the third aspect of the present invention in mine backfilling.

[0051] In some embodiments of the invention, the mine comprises fine-sized polymetallic tailings.

[0052] In some embodiments of the present invention, the fine-grained polymetallic tailings are lead-zinc ore classification tailings.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The cementitious material of the present invention can replace the traditional cementitious material. The filling body formed by the cementitious material has high compressive strength and high anti-seepage performance. Under the condition of the same lime-sand ratio, the compressive strength can reach 2 to 3 times that of cement, and the anti-seepage pressure is higher, that is, the anti-seepage performance is better. At the same time, the filling body formed has a lower leaching concentration of heavy metal ions and is more environmentally friendly.

[0055] (2) The main component of the cementitious material of the present invention is metallurgical solid waste from steel mills, which is low in cost and widely available, and can reduce production costs and meet the needs of large-scale production.

[0056] (3) The cementitious material of the present invention has excellent compressive strength and anti-seepage strength, and the formed filling body has a low heavy metal ion leaching concentration, and is suitable for use as a filling material and applied to mine backfill, especially the backfill of fine-grained polymetallic tailings. DETAILED DESCRIPTION

[0057] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0058] The compositions of the steel slag and slag used in the following examples and comparative examples of the present invention are as shown in Table 1:

[0059] Table 1 Main components of steel slag and slag

[0060] Solid Waste <![CDATA[Al2O3%]]> CaO% <![CDATA[SiO2%]]> <![CDATA[M Ca / M Si ]]> <![CDATA[M Al / M Si ]]> Vitreous mass content Steel slag 4.11 37.66 13.05 2.89 0.42 89% slag 14.56 40.16 33.04 1.33 0.89 92%

[0061] Among them, the percentage of oxide is mass percentage, M Ca / M Si and M Al / M Si is the molar ratio.

[0062] The slag is ground into slag powder, which meets the S95 grade slag powder requirements of GB / T18046-2017 "Granulated blast furnace slag powder for cement, mortar and concrete"; the steel slag is ground into steel slag powder, which meets the first grade requirements of GB / T20491-2017 "Steel slag powder for cement and concrete".

[0063] Steel slag, roasting dust removal ash, desulfurization ash and slag all come from Shaoguan Iron and Steel.

[0064] Table 2 Composition of roasting dust ash from Shaoguan Iron and Steel

[0065] Element CaO <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> <![CDATA[CaCO3]]> Mass content / % 68 8 3 1 20

[0066] Table 3 Main chemical composition of flue gas desulfurization ash from Shaoguan Iron and Steel Co., Ltd. semi-dry sintering process

[0067] Element Mass content / % Al2O3 0.167 CaO 51.506 Fe2O3 0.5918 K2O 0.3013 MgO 0.7192 Na2O 0.0501 SiO2 1.2435 P2O5 0.0097 SO3 14.822 Tl2O3 0.0001 Cl 1.6935

[0068] Note: Only the main ingredients are listed in Tables 1 and 3.

[0069] Activator: 90% by mass of Portland cement clinker and 10% by mass of water glass, mixed and ground into a specific surface area of ​​500±10m 2 / kg of powder, the moisture content is controlled to be no more than 1wt%.

[0070] The following describes it in conjunction with specific embodiments.

[0071] Example 1

[0072] This embodiment provides a cementitious material, comprising 25 parts of steel slag powder, 25 parts of roasting dust ash, 5 parts of desulfurization ash, 40 parts of slag powder, and 5 parts of activator; wherein the specific surface area of ​​the steel slag powder and the slag powder is 400±10m 2 / kg, moisture content is less than 1wt%.

[0073] The preparation method of the above-mentioned gelling material in this embodiment comprises the following steps:

[0074] The components were mixed in a gravity-free mixer for 30 minutes to obtain a gelling material.

[0075] Example 2

[0076] This embodiment provides a cementitious material, including 20 parts of steel slag powder, 20 parts of roasting dust ash, 10 parts of desulfurization ash, 45 parts of slag powder, and 5 parts of activator; wherein the specific surface area of ​​the steel slag powder and the slag powder is 450±10m 2 / kg, moisture content is less than 1wt%.

[0077] The preparation method of the cementitious material of this embodiment is the same as that of embodiment 1.

[0078] Test Case

[0079] The cementitious materials and aggregates obtained in Examples 1 and 2 were mixed with water to obtain a filling material to form a filling body. At the same time, cement (Yingde Taimu 425R cement) was used as a cementitious material to form a filling material with the same aggregate for comparison.

[0080] The tailings aggregates used in the test were all graded tailings from lead-zinc mines.

[0081] 1. Filling strength test:

[0082] (1) Preparation of slurry: first wipe the mixing blades and mixing barrel with a wet cloth, pour the mixing water into the mixing barrel, and then carefully add the weighed cementitious material and tailings into the water; start the mixer, and when the mixing is paused, scrape the slurry attached to the bottom and sides of the mixing barrel into the middle of the barrel. Stir slowly for 2 minutes and stir quickly for 1 minute to fully mix the slurry; when the mixing is completed, the slurry is ready for use;

[0083] (2) Molding: Stir the prepared slurry back and forth three times with a shovel, and then slowly pour the slurry into the test mold; load the mixed slurry into the mold in two layers, and the thickness of each layer is roughly equal, about half of the mold; the filled slurry should be slightly higher than the top surface of the mold to avoid shrinkage of the filled slurry after solidification, resulting in irregular specimens; when manually tamping, the mixture should be loaded into the test mold in two layers, and the thickness of each layer is roughly equal; the tamping of the test block should be carried out evenly from the edge to the center in a spiral direction. When tamping the bottom layer, the tamping rod should reach the bottom surface of the test mold, and when tamping the upper layer, the tamping rod should penetrate the lower layer with a depth of 20 to 30 mm. The tamping rod should be kept vertical and not tilted during tamping. At the same time, a spatula should be inserted along the inner wall of the test mold several times; the number of tamping times for each layer is 12 times; after tamping, gently tap the four sides of the test mold with a rubber hammer until the hole left by the tamping rod disappears, and scrape off the excess slurry and smooth it with a spatula;

[0084] (3) Demolding and curing: When the specimen is close to initial setting, remove the mold cover and carefully scrape the surface of the specimen with a putty knife; after the specimen is finally set, use a spray gun to demold, place neatly, and number the specimens; finally, cover the surface of the specimen with a waterproof film and place it in a curing room with a temperature of 20±2℃ and a humidity of ≥90% for curing; the specimens in the standard curing room are neatly placed on the bracket, with a spacing of 10 to 20 mm between each other, so that the surface of the specimens remains moist. The test results are shown in Tables 4 and 5;

[0085] Among them, the filling strength requirement of the filling mine room is: when the ash-sand ratio is 1:12, the strength shall not be less than 1.5MPa 7 days after filling, and the strength shall not be less than 3.0MPa 28 days after filling.

[0086] 2. Heavy metal leaching test: Tested in accordance with GB5085.3-2007 “Identification Standard for Leaching Toxicity of Hazardous Wastes”; the test results are shown in Table 6.

[0087] 3. Water-resistance test: Prepare the test specimens according to the filling strength test steps, and cure them in a standard curing room with a temperature of 20±2°C and a humidity of ≥90% for 3 days. Then, perform pore structure analysis on them by mercury intrusion porosimetry (MIP), and read the water-resistance pressure based on the mercury intrusion curve analysis; the greater the water-resistance pressure, the stronger the water-resistance performance; the test results are shown in Table 7.

[0088] The filling strength test results are shown in Table 4:

[0089] Table 4 Filling strength of different filling materials

[0090]

[0091] According to the results in Table 4, when cement is used as the cementitious material and the lime-sand ratio is 1:6, the 7d strength is only 1.8 MPa and the 28d strength is 2.8 MPa. However, when the cementitious material of Example 1 of the present invention is used, when the lime-sand ratio is 1:12 and the fluidity is better than that of cement slurry, the 7d strength reaches 2.3 MPa and the 28d strength can reach 3.4 MPa, which meets the mine's requirement that the 28d compressive strength of the mine filling reaches 3.0 MPa.

[0092] In addition, it can be seen from the results in Table 4 that the cementitious material of the present invention can still meet the mine filling quality standard when used in combination with different mine filling aggregates. The compressive performance that can be achieved by the cementitious material of the present invention is significantly higher than that of cement. Under the same lime-sand ratio, the compressive strength can reach 2 to 3 times that of cement.

[0093] Table 5 Comparison of cementitious material strength of Examples 1 and 2

[0094]

[0095]

[0096] In Table 5, the aggregate is tailings and the solid content is 78%.

[0097] The filling bodies formed by the cementitious materials of Examples 1 and 2 have high strength. This is because: the CaO contained in the roasted dust reacts with water during the filling process to form CaO+H2O=Ca(OH)2, providing an alkaline environment for the backfill colloid; in an alkaline environment, the CaSO4 in the desulfurized ash provides SO4 2- The synergistic stimulant forms a double excitation on the cementitious material of the present invention, and under the double excitation, the early strength and the later strength are guaranteed.

[0098] The unique properties of the cementitious material of the present invention in terms of fluidity, compressive strength and reduced water seepage can help improve the quality, reduce costs and increase efficiency of polymetallic tailings in filling mining. According to calculations, using the cementitious material of the present invention to replace cement can save cement usage and reduce the comprehensive filling cost by about 20%.

[0099] The heavy metal leaching test results are shown in Table 6 below.

[0100] The heavy metals contained in the polymetallic tailings enter the water environment or soil environment along with the surface water and groundwater, causing heavy metal pollution in the water environment and soil environment of the mining area and its surrounding areas. In the prior art, tailings are used as aggregates and cement cementitious materials are used as filling materials to backfill into the well to form a filling body. If the filling body has excessive heavy metal leaching in the underground environment, it will inevitably threaten the environmental safety of the mining area and the health of the workers. Therefore, the heavy metal leaching amount of the filling body formed by the cementitious material of Example 1 of the present invention and the cement filling body are compared in the following test, wherein the aggregates are all graded tailings and the ash-sand ratio is 1:8.

[0101] Table 6 Heavy metal leaching data of different filling materials

[0102]

[0103] It can be found from the data in Table 6 that the filling body formed by the cementitious material and tailings of the present invention has less heavy metal leaching than the filling body formed by cement and tailings, which is helpful for protecting groundwater.

[0104] The results of the anti-seepage performance test are shown in Table 7 below.

[0105] In the filling of polymetallic tailings mines, due to the high content of filling slurry and underground water, there are certain requirements for the anti-seepage performance of the filling body to prevent geological disasters caused by water seepage and the impact on mining production.

[0106] Table 7 Anti-seepage pressure of filling bodies formed by different filling materials

[0107]

[0108] As can be seen from Table 7, the impermeability of the filling body formed by the cementitious material and tailings of Example 1 is significantly better than that of the filling body formed by cement and tailings. In addition to being related to the amount of hydration products in the cementitious material and the network structure formed by it, the mechanical properties of the tailings filling body are most affected by the porosity and its distribution inside the filling body. The lower the porosity, the denser the structure, the higher the strength, and the stronger its impermeability. The impermeability of the filling body is directly related to its internal structure, especially to its critical pore size (dcr). By comparing the mercury injection curve, it is found that the use of the cementitious material of the present invention can reduce the porosity and void size of the tailings filling body, making its structure denser. At the same time, due to the increase in the degree of hydration, the pores inside it become smaller, that is, the dcr becomes smaller, thereby improving its impermeability.

[0109] In summary, the cementitious material of the present invention can replace traditional cementitious materials, and the backfill body formed by the cementitious material has high compressive strength and high impermeability. Under the condition of the same ash-sand ratio, the compressive strength can reach 2 to 3 times that of cement, and the impermeability pressure is higher, that is, the impermeability is better. At the same time, the leaching concentration of heavy metal ions is lower, which is more environmentally friendly, can also reduce production costs and meet the needs of large-scale production. It is suitable for filling materials and is applied to mine backfill, especially the backfill of fine-grained polymetallic tailings, and the tailings are mainly graded lead-zinc ore tailings.

[0110] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A cementitious material, It is characterized in that Calculated by mass, it includes the following components: 10-30 parts of steel slag, 5-30 parts of roasting dust ash, 3-10 parts of desulfurization ash, 30-50 parts of slag, and 5-10 parts of activator.

2. The gelling material according to claim 1, It is characterized in that The molar ratio of calcium to silicon in the steel slag is (2-4):1; And / or, the molar ratio of silicon to aluminum in the steel slag is (0.2-0.6):

1.

3. The gelling material according to claim 1, It is characterized in that The molar ratio of calcium to silicon in the slag is (1-3):1; And / or, the molar ratio of silicon to aluminum in the slag is (0.7-1):

1.

4. The gelling material according to claim 1 or 2, It is characterized in that The glass content in the steel slag is 80-95%.

5. The gelling material according to claim 1 or 3, It is characterized in that The glass content in the slag is 85-95%.

6. The gelling material according to claim 1, It is characterized in that The activator is a composite activator; the composite activator comprises a silicate activator and an alkaline activator.

7. A method for preparing the gelling material according to any one of claims 1 to 6, It is characterized in that The steps include: The cementitious material is obtained by mixing steel slag, roasting dust removal ash, desulfurization ash, slag and activator in proportion.

8. A filling material, It is characterized in that It comprises aggregate and cementitious material; the cementitious material is the cementitious material according to any one of claims 1 to 6.

9. The filling material according to claim 8, It is characterized in that The mass ratio of the cementitious material to the aggregate is 1:(4-12).

10. Use of the cementitious material according to any one of claims 1 to 6 or the filling material according to any one of claims 8 to 9 in mine backfilling.

Citation Information

Patent Citations

  • Cementing material containing waste incineration fly ash, steel slag and mineral slag, and preparation method and application thereof

    CN110818294A

  • Method for preparing mine filler by cementing solid wastes in iron and steel industry with heavy metal tailings

    CN112279565A

  • Preparation method of desulfurized fly ash cementing material

    CN114656171A

  • Cementing material for filling sulfur-containing metal mine as well as preparation method and application of cementing material

    CN116282980A

  • Method for preparing mine filling material using heavy metal tailings cemented by solid wastes in steel industry

    WO2022057104A1