Method for preparing harmless regenerated aggregate with excellent building performance by using slag

By crushing and harmless treatment of slag aggregate, combining the mixing of matrix asphalt and modifiers, hydrogen bonding is used to improve the bonding force, and metal separation is separated by high-temperature incineration and magnetic separation, the problem of slag landfill pollution is solved. It realizes harmless treatment and comprehensive utilization of resources, and improves the performance and recycling efficiency of recycled aggregates.

CN118908620APending Publication Date: 2024-11-08SHENZHEN XIJIANG ENVIRONMENTAL PROTECTION RESOURCES DEV & UTILIZATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411097532.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Because the slag contains harmful substances such as heavy metals, direct landfill will cause land pollution and cannot reuse resources, resulting in high treatment costs and waste of resources.

Method used

By obtaining the slag aggregate for crushing and harmless treatment, combining the mixing of matrix asphalt and modifier, hydrogen bonding is used to improve the bonding force, and metals are separated by high-temperature incineration and magnetic separation, combining heavy metal remover and microbial precipitation. Method to prepare harmless recycled aggregates with excellent building performance.

Benefits of technology

It improves the adhesion and stability of the recycled aggregate, realizes the comprehensive utilization of resources, reduces the amount of waste, reduces the treatment cost, and improves the recycling efficiency of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908620A_ABST
    Figure CN118908620A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of furnace slag waste reutilization, and discloses a method for preparing harmless regenerated aggregate with excellent building performance by utilizing furnace slag, and the method specifically comprises the following steps: S101, obtaining to-be-treated furnace slag, crushing the furnace slag to obtain furnace slag aggregate with the particle size of 100-500 microns, and performing harmless treatment on the furnace slag aggregate; s102, weighing 120-200 parts by weight of slag aggregate and 50-60 parts by weight of matrix asphalt, respectively adding the slag aggregate and the matrix asphalt into the modifier, heating the slag aggregate and the matrix asphalt, and continuously mechanically stirring the slag aggregate and the matrix asphalt for 30-50 minutes at the heating temperature of 80-100 DEG C to obtain initial bonding aggregate; s103, an air blowing pump is additionally arranged on one side of the stirring tank where the aggregate is initially bonded, and a large amount of external air is discharged into the stirring tank. Through the formation of hydrogen bonds, the binding power of the mixture of the matrix asphalt and the slag aggregate is increased by 2.2-2.5 times, and the molecular mass of the macromolecular substance is large, so that the substance generates more hydrogen bonds in the structure, and the binding power among the regenerated aggregates is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of slag waste recycling, and in particular to a method for producing harmless recycled aggregate with excellent building performance by utilizing slag. Background Art

[0002] Slag is mainly the residue after the incineration of domestic waste. The amount produced depends on the composition of the waste. Its main components are manganese oxide (MnO), silicon dioxide (SiO2), calcium oxide (CaO), aluminum oxide (A1203), iron oxide (Fe203), scrap metals, and a small amount of unburned organic matter.

[0003] At present, slag is directly landfilled and cannot be reused. Since slag contains harmful substances such as heavy metals, direct landfill will cause land pollution. Therefore, it needs to be harmlessly treated and then landfilled. This not only wastes resources, but also cannot reuse the slag, increasing the processing cost. Summary of the invention

[0004] The purpose of the present invention is to provide a method for producing harmless recycled aggregate with excellent construction performance using slag. Through the formation of hydrogen bonds, the bonding strength of the mixture of matrix asphalt and slag aggregate is increased by 1.2-1.5 times, and the molecular weight of the polymer substance is larger, so that the substance produces more hydrogen bonds in the structure, aiming to solve the problems in the prior art.

[0005] The present invention is achieved by using slag to produce harmless recycled aggregate with excellent building performance, which specifically includes the following steps:

[0006] S101: obtaining slag to be processed, crushing the slag to obtain slag aggregate with particles of 100-500 μm, and then performing harmless treatment on the slag aggregate;

[0007] S102: 120-200 parts of slag aggregate and 50-60 parts of matrix asphalt are weighed by weight, respectively added to the modifier, heated, and continuously stirred mechanically. The heating temperature is set to 80-100° C. and the stirring time is 30-50 minutes to obtain initial bonding aggregate;

[0008] S103: Add an air pump on one side of the mixing tank for initial bonding aggregate, discharge a large amount of external air into the mixing tank, and continuously heat and stir while filling with air to obtain airtight saturated bonding aggregate;

[0009] S103: Add 15-20 parts of stabilizer and 10-12 parts of surfactant to the airtight saturated bonding aggregate, let it stand for 5-10 minutes, and roll it every 10-15 minutes to obtain a stable airtight saturated bonding aggregate;

[0010] S104: adding 8-10 parts of rubber oil and 0.5-1.5 parts of electrolyte to the stable airtight saturated bonded aggregate, leaving it to stand for 15-20 minutes, and then performing centrifugal filtration to obtain dry bonded saturated aggregate;

[0011] S105: Spread the dry-bonded saturated aggregate on the ground and dry it naturally, so as to obtain the recycled aggregate which is harmless and has excellent construction performance made by using slag.

[0012] Furthermore, in S101, the slag aggregate is subjected to harmless treatment, including:

[0013] Placing the slag aggregate in a mixing container, and pouring water into the mixing container until the slag aggregate is completely submerged in water;

[0014] Adding a heavy metal remover to the mixed liquid and stirring continuously until the heavy metal remover and the mixed liquid are completely mixed, and recovering the heavy metal ions in the slag aggregate by the heavy metal remover;

[0015] The obtained heavy metal removal agent mixed liquid is sieved to recover the precipitated heavy metal ions.

[0016] Furthermore, the heavy metal remover is a heavy metal capture agent or a microbial colony. The heavy metal capture agent is a chemical agent that strongly chelates heavy metal ions, and its chemical reaction can better precipitate heavy metal ions. The microbial colony utilizes microbial metabolic activity to convert heavy metals in wastewater into water-insoluble substances to remove heavy metals in wastewater.

[0017] Furthermore, the slag aggregate is placed in a mixing container, and before water is injected into the mixing container, the elemental substances are removed, including:

[0018] The slag aggregate to be treated is placed in an incineration tank and incinerated at high temperature for 5-10 hours to completely oxidize, decompose and passivate the unburned substances in the slag aggregate;

[0019] The slag aggregate after high-temperature incineration is then subjected to magnetic separation to separate the metals and magnetic substances in the slag aggregate, which helps to recover resources.

[0020] Furthermore, in S102, the modifier is one or more of polyamide, polyacrylic acid, polyvinyl alcohol, polyurethane, and polybutylene acid.

[0021] Further, in S103, the gas is filled while being heated and stirred continuously to obtain an airtight saturated bonding aggregate, including:

[0022] The initial bonding aggregate is sheared by a shear mixer at a shear speed of 500-1000 r / min;

[0023] The air pump blows air into the shear opening of the initial bonding aggregate, and the operation is continuously circulated until the initial bonding aggregate becomes fluffy, thereby obtaining an airtight saturated bonding aggregate.

[0024] Furthermore, the stabilizer is composed of two or three of polyvinyl alcohol, cellulose and ethylene glycol.

[0025] Further, in S104, the rubber oil comprises the following components in parts by weight: 20-25 parts of polyethylene grease, 10-20 parts of matting powder, 35-45 parts of ethyl acetate, 10-30 parts of n-butyl acetate, and 25-35 parts of diacetone alcohol.

[0026] Furthermore, by centrifuging the stable airtight saturated bonded aggregate, excess liquid grease in the stable airtight saturated bonded aggregate is removed, and the sieve hole diameter in the centrifugal equipment for the centrifugal treatment is set to 50-80 μm. During centrifugation, excess liquid grease passes through the sieve holes and is separated from the stable airtight saturated bonded aggregate.

[0027] Further, in S105, the dry-bonded saturated aggregate is spread on the ground for natural drying, including:

[0028] The obtained dry bonded saturated aggregate is separated from the centrifugal device and placed on a drying rack for air drying for 7-10 days to completely remove the moisture that has infiltrated the slag aggregate when the slag aggregate is mixed with water.

[0029] Compared with the prior art, the method provided by the present invention for producing harmless recycled aggregate with excellent building performance by using slag has the following beneficial effects:

[0030] 1. After the slag is treated with high temperature harmlessness and then separated from scrap metals such as scrap steel by magnetic separation, the slag can be comprehensively utilized by mixing the slag aggregate with matrix asphalt and modifier. Since the modifiers are all high molecular substances formed by polycondensation reaction of polyamide, polyacrylic acid, etc., and these high molecular substances contain hydrogen bonds, after mixing with the matrix asphalt, the bonding force of the mixture of matrix asphalt and slag aggregate is increased by 2.2-2.5 times through the formation of hydrogen bonds. In addition, the molecular weight of the high molecular substance is relatively large, so that the substance produces more hydrogen bonds in the structure, thereby improving the bonding force between the recycled aggregates;

[0031] 2. The addition of stabilizers improves the internal stability of recycled aggregates, mainly polyvinyl alcohol, cellulose, and ethylene glycol. These substances are not easy to react chemically, which increases the temperature range that recycled aggregates can withstand by 50°C, avoiding expansion or cracking of recycled aggregates during high-temperature processing. At the same time, it also makes the performance of the road surface subsequently paved with recycled aggregate materials more stable.

[0032] Specifically, high temperature treatment: through high temperature incineration, the harmful substances in the slag are thoroughly oxidized, decomposed and passivated, thereby reducing the harm to the environment.

[0033] Magnetic separation and screening: Magnetic separation technology is used to separate metals and other useful materials from slag, which not only helps resource recovery but also reduces the volume and complexity of final disposal.

[0034] Comprehensive utilization: Slag can be used as a paving base, a landfill cover, or to make unburned bricks. This comprehensive utilization not only reduces the amount of waste, but also increases the recycling of resources.

[0035] There are mainly the following methods for harmless treatment:

[0036] 1. Heavy metal ion adsorption method

[0037] Heavy metal scavengers can be directly added to wastewater. They are chemical agents that can strongly chelate heavy metal ions. Their chemical reactions can better precipitate heavy metal ions (copper, nickel, lead, zinc, cadmium, etc.) so that the wastewater meets the discharge standards.

[0038] 2. Biological precipitation method

[0039] The biological precipitation method mainly utilizes the metabolic activity of microorganisms to convert heavy metals in wastewater into water-insoluble substances to remove heavy metals in wastewater. The microorganisms used in the biological precipitation method are mainly sulfate-reducing bacteria; under anaerobic conditions, reduced sulfate can convert sulfate into sulfide ions, resulting in the precipitation of insoluble metal sulfides. Since most of the heavy metals in wastewater exist in the form of sulfate, the purpose of "waste utilization" can be achieved. In addition, it also has the characteristics of multiple heavy metal treatment, thorough treatment, and great treatment potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A schematic flow chart of a method for producing harmless recycled aggregate with excellent building performance using slag proposed by the present invention;

[0041] Figure 2 A schematic flow chart of a method for producing harmless recycled aggregate with excellent building performance by utilizing slag, and then performing harmless treatment on the slag aggregate, as proposed by the present invention;

[0042] Figure 3 The present invention provides a method for producing harmless recycled aggregate with excellent construction performance by utilizing slag, which is provided by the present invention, and is characterized in that the method is continuously heated and stirred while being filled with air to obtain airtight saturated bonded aggregate. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0044] The implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0045] The same or similar numbers in the drawings of this embodiment correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right" and the like indicate directions or positional relationships based on the directions or positional relationships shown in the drawings, it is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, the terms describing the positional relationship in the drawings are only used for illustrative purposes and cannot be understood as limitations on the present invention. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.

[0046] Example 1

[0047] Reference Figure 1-3 As shown, a method for making harmless recycled aggregate with excellent building performance using slag specifically comprises the following steps:

[0048] S101: obtaining slag to be processed, crushing the slag to obtain slag aggregate with particles of 100 μm, and then performing harmless treatment on the slag aggregate;

[0049] S102: 120 parts of slag aggregate and 50 parts of matrix asphalt are weighed by weight, added to the modifier, heated, and continuously stirred mechanically. The heating temperature is set to 80° C. and the stirring time is 30 minutes to obtain initial bonding aggregate;

[0050] S103: Add an air pump on one side of the mixing tank for initial bonding aggregate, discharge a large amount of external air into the mixing tank, and continuously heat and stir while filling with air to obtain airtight saturated bonding aggregate;

[0051] S103: add 15 parts of stabilizer and 10 parts of surfactant to the airtight saturated bonding aggregate, let it stand for 5 minutes, and roll it every 10 minutes to obtain a stable airtight saturated bonding aggregate;

[0052] S104: Add 8 parts of rubber oil and 0.5 parts of electrolyte to the stable airtight saturated bonded aggregate, let it stand for 15 minutes, and then perform centrifugal filtration to obtain dry bonded saturated aggregate:

[0053] S105: Spread the dry-bonded saturated aggregate on the ground and dry it naturally, so as to obtain the recycled aggregate which is harmless and has excellent construction performance made by using slag.

[0054] In S101, the slag aggregate is then subjected to harmless treatment, including:

[0055] Placing the slag aggregate in a mixing container, and pouring water into the mixing container until the slag aggregate is completely submerged in water;

[0056] Adding a heavy metal remover to the mixed liquid and stirring continuously until the heavy metal remover and the mixed liquid are completely mixed, and recovering the heavy metal ions in the slag aggregate by the heavy metal remover;

[0057] The obtained heavy metal removal agent mixed liquid is sieved to recover the precipitated heavy metal ions.

[0058] Heavy metal removers are heavy metal capture agents or microbial colonies. Heavy metal capture agents are chemical agents that strongly chelate heavy metal ions. Their chemical reactions can precipitate heavy metal ions well. Microbial colonies utilize microbial metabolic activity to convert heavy metals in wastewater into water-insoluble substances to remove heavy metals from wastewater.

[0059] Place the slag aggregate in a mixing container and remove the elemental substances before adding water to the mixing container, including:

[0060] The slag aggregate to be treated is placed in an incineration tank and incinerated at high temperature for 5 hours to completely oxidize, decompose and passivate the unburned substances in the slag aggregate;

[0061] The slag aggregate after high-temperature incineration is then subjected to magnetic separation to separate the metals and magnetic substances in the slag aggregate, which helps to recover resources.

[0062] The modifier is polyamide.

[0063] In S103, the gas is filled while being heated and stirred continuously to obtain an airtight saturated bonding aggregate, including:

[0064] The initial bonding aggregate was sheared using a shear mixer at a shear rate of 500 r / min;

[0065] The air pump blows air into the shear opening of the initial bonding aggregate, and the operation is continuously circulated until the initial bonding aggregate becomes fluffy, thereby obtaining an airtight saturated bonding aggregate.

[0066] The stabilizer is polyvinyl alcohol and cellulose, with a mixing ratio of 1:1.

[0067] In S104, the rubber oil includes the following components by weight: 20 parts of polyethylene resin, 10 parts of matting powder, 35 parts of ethyl acetate, 10 parts of n-butyl acetate, and 25 parts of diacetone alcohol.

[0068] The stable airtight saturated bonded aggregate is centrifuged to remove excess liquid grease in the stable airtight saturated bonded aggregate. The sieve hole diameter in the centrifugal device for centrifugal treatment is set to 50μm. During centrifugation, the excess liquid grease passes through the sieve holes and is separated from the stable airtight saturated bonded aggregate.

[0069] In S105, the dry-bonded saturated aggregate is spread on the ground for natural drying, including:

[0070] The obtained dry bonded saturated aggregate is separated from the centrifugal device and placed on a drying rack for air drying for 7 days to completely remove the moisture that has infiltrated the slag aggregate when the slag aggregate is mixed with water.

[0071] Example 2

[0072] Reference Figure 1-3 As shown, a method for making harmless recycled aggregate with excellent building performance using slag specifically comprises the following steps:

[0073] S101: obtaining slag to be processed, crushing the slag to obtain slag aggregate with particles of 200 μm, and then performing harmless treatment on the slag aggregate;

[0074] S102: 140 parts of slag aggregate and 55 parts of matrix asphalt are weighed by weight, respectively added to the modifier, heated, and continuously stirred mechanically. The heating temperature is set to 90° C. and the stirring time is 40 minutes to obtain initial bonding aggregate;

[0075] S103: Add an air pump on one side of the mixing tank for initial bonding aggregate, discharge a large amount of external air into the mixing tank, and continuously heat and stir while filling with air to obtain airtight saturated bonding aggregate;

[0076] S103: add 16 parts of stabilizer and 11 parts of surfactant to the airtight saturated bonding aggregate, let it stand for 8 minutes, and roll it every 12 minutes to obtain a stable airtight saturated bonding aggregate;

[0077] S104: adding 9 parts of rubber oil and 1 part of electrolyte to the stable airtight saturated bonded aggregate, standing for 17 minutes, and then centrifugally filtering to obtain dry bonded saturated aggregate;

[0078] S105: Spread the dry-bonded saturated aggregate on the ground and dry it naturally, so as to obtain the recycled aggregate which is harmless and has excellent construction performance made by using slag.

[0079] In S101, the slag aggregate is then subjected to harmless treatment, including:

[0080] Placing the slag aggregate in a mixing container, and pouring water into the mixing container until the slag aggregate is completely submerged in water;

[0081] Adding a heavy metal remover to the mixed liquid and stirring continuously until the heavy metal remover and the mixed liquid are completely mixed, and recovering the heavy metal ions in the slag aggregate by the heavy metal remover;

[0082] The obtained heavy metal removal agent mixed liquid is sieved to recover the precipitated heavy metal ions.

[0083] Heavy metal removers are heavy metal capture agents or microbial colonies. Heavy metal capture agents are chemical agents that strongly chelate heavy metal ions. Their chemical reactions can precipitate heavy metal ions well. Microbial colonies utilize microbial metabolic activity to convert heavy metals in wastewater into water-insoluble substances to remove heavy metals from wastewater.

[0084] Place the slag aggregate in a mixing container and remove the elemental substances before adding water to the mixing container, including:

[0085] The slag aggregate to be treated is placed in an incineration tank and incinerated at high temperature for 8 hours to completely oxidize, decompose and passivate the unburned substances in the slag aggregate;

[0086] The slag aggregate after high-temperature incineration is then subjected to magnetic separation to separate the metals and magnetic substances in the slag aggregate, which helps to recover resources.

[0087] The modifier is polyamide and polyacrylic acid, with a mixing ratio of 1:1.

[0088] In S103, the gas is filled while being heated and stirred continuously to obtain an airtight saturated bonding aggregate, including:

[0089] The initial bonding aggregate is sheared by a shear mixer at a shear speed of 600 r / min;

[0090] The air pump blows air into the shear opening of the initial bonding aggregate, and the operation is continuously circulated until the initial bonding aggregate becomes fluffy, thereby obtaining an airtight saturated bonding aggregate.

[0091] The stabilizer is polyvinyl alcohol, cellulose, and ethylene glycol, with a mixing ratio of 1:1:1.

[0092] In S104, the rubber oil includes the following components by weight: 22 parts of polyethylene resin, 12 parts of matting powder, 38 parts of ethyl acetate, 25 parts of n-butyl acetate, and 25 parts of diacetone alcohol.

[0093] The stable airtight saturated bonded aggregate is centrifuged to remove excess liquid grease in the stable airtight saturated bonded aggregate. The sieve hole diameter in the centrifugal device for centrifugal treatment is set to 60μm. During centrifugation, the excess liquid grease passes through the sieve holes and is separated from the stable airtight saturated bonded aggregate.

[0094] In S105, the dry-bonded saturated aggregate is spread on the ground for natural drying, including:

[0095] The obtained dry bonded saturated aggregate is separated from the centrifugal device and placed on a drying rack for air drying for 8 days to completely remove the moisture that has infiltrated the slag aggregate when the slag aggregate is mixed with water.

[0096] Example 3

[0097] Reference Figure 1-3 As shown, a method for making harmless recycled aggregate with excellent building performance using slag specifically comprises the following steps:

[0098] S101: obtaining slag to be processed, crushing the slag to obtain slag aggregate with particles of 300 μm, and then performing harmless treatment on the slag aggregate;

[0099] S102: 170 parts of slag aggregate and 55 parts of matrix asphalt are weighed by weight, respectively added to the modifier, heated, and continuously stirred mechanically. The heating temperature is set to 90° C. and the stirring time is 40 minutes to obtain initial bonding aggregate;

[0100] S103: Add an air pump on one side of the mixing tank for initial bonding aggregate, discharge a large amount of external air into the mixing tank, and continuously heat and stir while filling with air to obtain airtight saturated bonding aggregate;

[0101] S1 03: Add 18 parts of stabilizer and 11 parts of surfactant to the airtight saturated bonding aggregate, let it stand for 7 minutes, and roll it every 12 minutes to obtain a stable airtight saturated bonding aggregate;

[0102] S104: adding 9 parts of rubber oil and 1 part of electrolyte to the stable airtight saturated bonded aggregate, leaving it to stand for 18 minutes, and then performing centrifugal filtration to obtain dry bonded saturated aggregate;

[0103] S105: Spread the dry-bonded saturated aggregate on the ground and dry it naturally, so as to obtain the recycled aggregate which is harmless and has excellent construction performance made by using slag.

[0104] In S101, the slag aggregate is then subjected to harmless treatment, including:

[0105] Placing the slag aggregate in a mixing container, and pouring water into the mixing container until the slag aggregate is completely submerged in water;

[0106] Adding a heavy metal remover to the mixed liquid and stirring continuously until the heavy metal remover and the mixed liquid are completely mixed, and recovering the heavy metal ions in the slag aggregate by the heavy metal remover;

[0107] The obtained heavy metal removal agent mixed liquid is sieved to recover the precipitated heavy metal ions.

[0108] Heavy metal removers are heavy metal capture agents or microbial colonies. Heavy metal capture agents are chemical agents that strongly chelate heavy metal ions. Their chemical reactions can precipitate heavy metal ions well. Microbial colonies utilize microbial metabolic activity to convert heavy metals in wastewater into water-insoluble substances to remove heavy metals from wastewater.

[0109] Place the slag aggregate in a mixing container and remove the elemental substances before adding water to the mixing container, including:

[0110] The slag aggregate to be treated is placed in an incineration tank and incinerated at high temperature for 8 hours to completely oxidize, decompose and passivate the unburned substances in the slag aggregate;

[0111] The slag aggregate after high-temperature incineration is then subjected to magnetic separation to separate the metals and magnetic substances in the slag aggregate, which helps to recover resources.

[0112] The modifiers are polyvinyl alcohol, polyurethane and polybutylene acid, and the mixing ratio is 1:1:1.

[0113] In S103, the gas is filled while being heated and stirred continuously to obtain an airtight saturated bonding aggregate, including:

[0114] The initial bonding aggregate is sheared by a shear mixer at a shear speed of 800 r / min;

[0115] The air pump blows air into the shear opening of the initial bonding aggregate, and the operation is continuously circulated until the initial bonding aggregate becomes fluffy, thereby obtaining an airtight saturated bonding aggregate.

[0116] The stabilizer is cellulose and ethylene glycol, with a mixing ratio of 1:2.

[0117] In S104, the rubber oil includes the following components by weight: 22 parts of polyethylene resin, 16 parts of matting powder, 40 parts of ethyl acetate, 20 parts of n-butyl acetate, and 30 parts of diacetone alcohol.

[0118] The stable airtight saturated bonded aggregate is centrifuged to remove excess liquid grease in the stable airtight saturated bonded aggregate. The sieve hole diameter in the centrifugal device for centrifugal treatment is set to 70 μm. During centrifugation, the excess liquid grease passes through the sieve holes and is separated from the stable airtight saturated bonded aggregate.

[0119] In S105, the dry-bonded saturated aggregate is spread on the ground for natural drying, including:

[0120] The obtained dry bonded saturated aggregate is separated from the centrifugal device and placed on a drying rack for air drying for 9 days to completely remove the moisture that has infiltrated the slag aggregate when the slag aggregate is mixed with water.

[0121] Example 4

[0122] Reference Figure 1-3 As shown, a method for making harmless recycled aggregate with excellent building performance using slag specifically comprises the following steps:

[0123] S101: obtaining slag to be processed, crushing the slag to obtain slag aggregate with particles of 400 μm, and then performing harmless treatment on the slag aggregate;

[0124] S102: 180 parts of slag aggregate and 57 parts of matrix asphalt are weighed by weight, added to the modifier, heated, and continuously stirred mechanically. The heating temperature is set to 95°C and the stirring time is 45 minutes to obtain the initial bonding aggregate:

[0125] S103: Add an air pump on one side of the mixing tank for initial bonding aggregate, discharge a large amount of external air into the mixing tank, and continuously heat and stir while filling with air to obtain airtight saturated bonding aggregate;

[0126] S103: add 18 parts of stabilizer and 11 parts of surfactant to the airtight saturated bonding aggregate, let it stand for 8 minutes, and roll it every 13 minutes to obtain a stable airtight saturated bonding aggregate;

[0127] S104: adding 9 parts of rubber oil and 1 part of electrolyte to the stable airtight saturated bonded aggregate, leaving it to stand for 18 minutes, and then performing centrifugal filtration to obtain dry bonded saturated aggregate;

[0128] S1 05: Spread the dry-bonded saturated aggregate on the ground and dry it naturally, so as to obtain the recycled aggregate which is harmless and has excellent construction performance made by using slag.

[0129] In S101, the slag aggregate is then subjected to harmless treatment, including:

[0130] Placing the slag aggregate in a mixing container, and pouring water into the mixing container until the slag aggregate is completely submerged in water;

[0131] Adding a heavy metal remover to the mixed liquid and stirring continuously until the heavy metal remover and the mixed liquid are completely mixed, and recovering the heavy metal ions in the slag aggregate by the heavy metal remover;

[0132] The obtained heavy metal removal agent mixed liquid is sieved to recover the precipitated heavy metal ions.

[0133] Heavy metal removers are heavy metal capture agents or microbial colonies. Heavy metal capture agents are chemical agents that strongly chelate heavy metal ions. Their chemical reactions can precipitate heavy metal ions well. Microbial colonies utilize microbial metabolic activity to convert heavy metals in wastewater into water-insoluble substances to remove heavy metals from wastewater.

[0134] Place the slag aggregate in a mixing container and remove the elemental substances before adding water to the mixing container, including:

[0135] The slag aggregate to be treated is placed in an incineration tank and incinerated at high temperature for 8 hours to completely oxidize, decompose and passivate the unburned substances in the slag aggregate;

[0136] The slag aggregate after high-temperature incineration is then subjected to magnetic separation to separate the metals and magnetic substances in the slag aggregate, which helps to recover resources.

[0137] The modifier is polyamide, polyacrylic acid, polyvinyl alcohol, polyurethane and polybutylene acid in a mixing ratio of 1: :2:1:1.

[0138] In S103, the gas is filled while being heated and stirred continuously to obtain an airtight saturated bonding aggregate, including:

[0139] The initial bonding aggregate was sheared by a shear mixer at a shear speed of 900 r / min;

[0140] The air pump blows air into the shear opening of the initial bonding aggregate, and the operation is continuously circulated until the initial bonding aggregate becomes fluffy, thereby obtaining an airtight saturated bonding aggregate.

[0141] The stabilizer is polyvinyl alcohol, cellulose, and ethylene glycol, with a mixing ratio of 1:2:1.

[0142] In S104, the rubber oil includes the following components by weight: 23 parts of polyethylene resin, 17 parts of matting powder, 40 parts of ethyl acetate, 25 parts of n-butyl acetate, and 30 parts of diacetone alcohol.

[0143] The stable airtight saturated bonded aggregate is centrifuged to remove excess liquid grease in the stable airtight saturated bonded aggregate. The sieve hole diameter in the centrifugal device for centrifugal treatment is set to 75μm. During centrifugation, the excess liquid grease passes through the sieve holes and is separated from the stable airtight saturated bonded aggregate.

[0144] In S105, the dry-bonded saturated aggregate is spread on the ground for natural drying, including:

[0145] The obtained dry bonded saturated aggregate is separated from the centrifugal device and placed on a drying rack for air drying for 9 days to completely remove the moisture that has infiltrated the slag aggregate when the slag aggregate is mixed with water.

[0146] Example 5

[0147] Reference Figure 1-3 As shown, a method for making harmless recycled aggregate with excellent building performance using slag specifically comprises the following steps:

[0148] S101: obtaining slag to be processed, crushing the slag to obtain slag aggregate with particles of 500 μm, and then performing harmless treatment on the slag aggregate;

[0149] S102: 200 parts of slag aggregate and 60 parts of matrix asphalt are weighed by weight, respectively added to the modifier, heated, and continuously stirred mechanically. The heating temperature is set to 100° C. and the stirring time is 50 minutes to obtain initial bonding aggregate;

[0150] S103: Add an air pump on one side of the mixing tank for initial bonding aggregate, discharge a large amount of external air into the mixing tank, and continuously heat and stir while filling with air to obtain airtight saturated bonding aggregate;

[0151] S103: Add 20 parts of stabilizer and 12 parts of surfactant to the airtight saturated bonding aggregate, let it stand for 10 minutes, and roll it every 15 minutes to obtain a stable airtight saturated bonding aggregate;

[0152] S104: adding 10 parts of rubber oil and 1.5 parts of electrolyte to the stable airtight saturated bonded aggregate, leaving it to stand for 20 minutes, and then performing centrifugal filtration to obtain dry bonded saturated aggregate;

[0153] S105: Spread the dry-bonded saturated aggregate on the ground and dry it naturally, so as to obtain the recycled aggregate which is harmless and has excellent construction performance made by using slag.

[0154] In S101, the slag aggregate is then subjected to harmless treatment, including:

[0155] Placing the slag aggregate in a mixing container, and pouring water into the mixing container until the slag aggregate is completely submerged in water;

[0156] Add heavy metal remover to the mixed liquid and stir continuously until the heavy metal remover and the mixed liquid are completely mixed, and the heavy metal ions in the slag aggregate are recovered by the heavy metal remover:

[0157] The obtained heavy metal removal agent mixed liquid is sieved to recover the precipitated heavy metal ions.

[0158] Heavy metal removers are heavy metal capture agents or microbial colonies. Heavy metal capture agents are chemical agents that strongly chelate heavy metal ions. Their chemical reactions can precipitate heavy metal ions well. Microbial colonies utilize microbial metabolic activity to convert heavy metals in wastewater into water-insoluble substances to remove heavy metals from wastewater.

[0159] Place the slag aggregate in a mixing container and remove the elemental substances before adding water to the mixing container, including:

[0160] The slag aggregate to be treated is placed in an incineration tank and incinerated at high temperature for 10 hours to completely oxidize, decompose and passivate the unburned substances in the slag aggregate;

[0161] The slag aggregate after high-temperature incineration is then subjected to magnetic separation to separate the metals and magnetic substances in the slag aggregate, which helps to recover resources.

[0162] The modifiers are polyamide, polyacrylic acid, polyvinyl alcohol and polyurethane, and the mixing ratio is 2:2:1:2.

[0163] In S103, the gas is filled while being heated and stirred continuously to obtain an airtight saturated bonding aggregate, including:

[0164] The initial bonding aggregate is sheared by a shear mixer at a shear speed of 1000 r / min;

[0165] The air pump blows air into the shear opening of the initial bonding aggregate, and the operation is continuously circulated until the initial bonding aggregate becomes fluffy, thereby obtaining an airtight saturated bonding aggregate.

[0166] The stabilizer is polyvinyl alcohol and ethylene glycol, with a mixing ratio of 1:2.

[0167] In S104, the rubber oil includes the following components by weight: 25 parts of polyethylene resin, 20 parts of matting powder, 45 parts of ethyl acetate, 30 parts of n-butyl acetate, and 35 parts of diacetone alcohol.

[0168] The stable airtight saturated bonded aggregate is centrifuged to remove excess liquid grease in the stable airtight saturated bonded aggregate. The sieve hole diameter in the centrifugal device for centrifugal treatment is set to 80 μm. During centrifugation, the excess liquid grease passes through the sieve holes and is separated from the stable airtight saturated bonded aggregate.

[0169] In S105, the dry-bonded saturated aggregate is spread on the ground for natural drying, including:

[0170] The obtained dry bonded saturated aggregate is separated from the centrifugal device and placed on a drying rack for air drying for 10 days to completely remove the moisture that has infiltrated the slag aggregate when the slag aggregate is mixed with water.

[0171] Experimental example

[0172] The recycled aggregates prepared in Examples 1-5 are now compared with the slag of the prior art (comparative example), and the comparison results are shown in the following table:

[0173]

[0174] The above table is a performance test table of recycled aggregate of Examples 1-5 and the control group. It can be seen from the table that the bonding force in Examples 1-5 is increased by 2.2-2.5 times compared with the control group, the compressive strength is slightly increased by more than 50%, and the heat resistance temperature is also increased by more than 50°C, which avoids the expansion or cracking of the recycled aggregate during high-temperature processing, and also makes the performance of the road surface subsequently paved with the recycled aggregate material more stable.

[0175] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing harmless recycled aggregate with excellent building performance using slag, characterized in that: The specific steps include: S101: obtaining slag to be processed, crushing the slag to obtain slag aggregate with particles of 100-500 μm, and then performing harmless treatment on the slag aggregate; S102: 120-200 parts of slag aggregate and 50-60 parts of matrix asphalt are weighed by weight, respectively added to the modifier, heated, and continuously stirred mechanically. The heating temperature is set to 80-100° C. and the stirring time is 30-50 minutes to obtain initial bonding aggregate; S103: Add an air pump on one side of the mixing tank of the initial bonding aggregate to discharge a large amount of external air into the mixing tank, and continuously heat and stir while filling the tank to obtain airtight saturated bonding aggregate, then add 15-20 parts of stabilizer and 10-12 parts of surfactant to the airtight saturated bonding aggregate, let it stand for 5-10 minutes, and roll it every 10-15 minutes to obtain stable airtight saturated bonding aggregate; S104: adding 8-10 parts of rubber oil and 0.5-1.5 parts of electrolyte to the stable airtight saturated bonded aggregate, leaving it to stand for 15-20 minutes, and then performing centrifugal filtration to obtain dry bonded saturated aggregate; S105: Spread the dry-bonded saturated aggregate on the ground and dry it naturally, so as to obtain the recycled aggregate which is harmless and has excellent construction performance made by using slag.

2. A method for producing harmless recycled aggregate with excellent building performance using slag as claimed in claim 1, characterized in that: In S101, the slag aggregate is then subjected to harmless treatment, including: Placing the slag aggregate in a mixing container, and pouring water into the mixing container until the slag aggregate is completely submerged in water; Adding a heavy metal remover to the mixed liquid and stirring continuously until the heavy metal remover and the mixed liquid are completely mixed, and recovering the heavy metal ions in the slag aggregate by the heavy metal remover; The obtained heavy metal removal agent mixed liquid is sieved to recover the precipitated heavy metal ions.

3. A method for producing harmless recycled aggregate with excellent construction performance using slag as claimed in claim 2, characterized in that: The heavy metal remover is a heavy metal capture agent or a microbial colony. The heavy metal capture agent is a chemical agent that strongly chelates heavy metal ions, and its chemical reaction can better precipitate heavy metal ions. The microbial colony utilizes microbial metabolic activity to convert heavy metals in wastewater into water-insoluble substances to remove heavy metals in wastewater.

4. A method for producing harmless recycled aggregate with excellent construction performance using slag as claimed in claim 3, characterized in that: Place the slag aggregate in a mixing container and remove the elemental substances before adding water to the mixing container, including: The slag aggregate to be treated is placed in an incineration tank and incinerated at high temperature for 5-10 hours to completely oxidize, decompose and passivate the unburned substances in the slag aggregate; The slag aggregate after high-temperature incineration is then subjected to magnetic separation to separate the metals and magnetic substances in the slag aggregate, which helps to recover resources.

5. A method for producing harmless recycled aggregate with excellent construction performance using slag as claimed in claim 4, characterized in that: In S102, the modifier is one or more of polyamide, polyacrylic acid, polyvinyl alcohol, polyurethane, and polybutylene acid.

6. A method for producing harmless recycled aggregate with excellent construction performance using slag as claimed in claim 5, characterized in that: In S103, the gas is filled while being heated and stirred continuously to obtain an airtight saturated bonding aggregate, including: The initial bonding aggregate is sheared by a shear mixer at a shear speed of 500-1000 r / min; The air pump blows air into the shear opening of the initial bonding aggregate, and the operation is continuously circulated until the initial bonding aggregate becomes fluffy, thereby obtaining an airtight saturated bonding aggregate.

7. A method for producing harmless recycled aggregate with excellent construction performance using slag as claimed in claim 6, characterized in that: The stabilizer is composed of two or three of polyvinyl alcohol, cellulose and ethylene glycol.

8. A method for producing harmless recycled aggregate with excellent construction performance using slag as claimed in claim 7, characterized in that: In S104, the rubber oil comprises the following components in parts by weight: 20-25 parts of polyethylene resin, 10-20 parts of matting powder, 35-45 parts of ethyl acetate, 10-30 parts of n-butyl acetate, and 25-35 parts of diacetone alcohol.

9. A method for producing harmless recycled aggregate with excellent construction performance using slag as claimed in claim 8, characterized in that: By centrifuging the stable airtight saturated bonded aggregate, excess liquid grease in the stable airtight saturated bonded aggregate is removed. The sieve hole diameter in the centrifugal device for the centrifugal treatment is set to 50-80μm. During centrifugation, excess liquid grease passes through the sieve holes and is separated from the stable airtight saturated bonded aggregate.

10. A method for producing harmless recycled aggregate with excellent construction performance using slag as claimed in claim 9, characterized in that: In S105, the dry-bonded saturated aggregate is spread on the ground for natural drying, including: The obtained dry bonded saturated aggregate is separated from the centrifugal device and placed on a drying rack for air drying for 7-10 days to completely remove the moisture that has infiltrated the slag aggregate when the slag aggregate is mixed with water.