Composite high-modulus agent for anti-rutting asphalt pavement and preparation method of composite high-modulus agent

By using a composite high-modulus agent composed of recycled asphalt pavement milling material and composite high-modulus modified asphalt, the problems of poor compatibility between high-modulus agents and asphalt and high cost have been solved, improving the rutting resistance and low-temperature performance of asphalt pavement, and realizing the recycling of materials and environmentally friendly production.

CN118908628APending Publication Date: 2024-11-08JIANGSU JUDENG CONSTR ENG CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410956299.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing high modulus agents have poor compatibility with asphalt, resulting in insufficient cohesiveness of asphalt mixtures, which affects low-temperature performance and fatigue performance. At the same time, they are costly, and old asphalt pavement materials are not effectively recycled.

Method used

The main raw material is recycled powder from milled old asphalt pavement. It is combined with composite high modulus modified asphalt, polyethylene wax, fiber and asphalt deodorizing agent to form a composite high modulus agent. It is prepared through a specific process to form a network winding structure to improve the crack resistance, shear resistance, compressive strength and impact resistance of asphalt mixture.

Benefits of technology

It improves the rutting resistance and low-temperature crack resistance of asphalt pavement, while reducing harmful gas emissions and costs during the production process, and realizes material recycling and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908628A_ABST
    Figure CN118908628A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of road engineering materials, and relates to a high-modulus agent, in particular to a composite high-modulus agent for an anti-rutting asphalt pavement and a preparation method of the composite high-modulus agent. The composite high-modulus agent comprises the following raw materials in parts by mass: 50%-70% of old asphalt pavement milling material recycled powder, 5%-15% of composite high-modulus modified asphalt, 3%-10% of polyethylene wax, 2%-5% of solvent oil, 5%-8% of fibers, 0.1%-0.5% of an asphalt deodorant and 10%-15% of high molecular weight polyethylene, wherein the total mass of the raw materials is 100%. The composite high-modulus agent does not reduce the low-temperature crack resistance and water damage resistance of an asphalt mixture on the premise of improving the modulus of an asphalt pavement and improving the rutting resistance, and meanwhile, has the characteristics of low cost, environment friendliness, convenience in use, convenience in popularization and application and the like.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] (Zhang Hao, Yang Feng, Xiao Hubing, Hu Chun) Technical Field

[0002] The invention belongs to the field of road engineering materials and relates to a high modulus agent, in particular to a composite high modulus agent for rutting-resistant asphalt pavement and a preparation method thereof, which has the characteristics of outstanding performance, green and low carbon, recyclable and environmentally friendly, low cost and easy use. Technical Background

[0003] With the increasing traffic volume on my country's expressways and the characteristics of large axle loads and channelized traffic, asphalt pavements are prone to significant permanent deformation and accumulated rutting under high temperature and continuous load. The appearance of rutting on asphalt pavements seriously affects the service quality and driving safety of high-grade pavements, and directly affects the service life of asphalt pavements, resulting in increased maintenance costs and posing a safety hazard to transportation.

[0004] In response to this problem, road workers at home and abroad have carried out a series of research work. In terms of material additives, a series of technologies such as high modulus asphalt mixture, low-grade asphalt mixture, anti-rutting agent, high modulus agent, etc. are used, all of which aim to improve the road surface's ability to resist deformation. In most parts of my country, increasing the modulus of asphalt mixture under high temperature conditions can effectively slow down the occurrence of rutting. However, in some areas with cold winters and rainy summers, simply increasing the modulus of asphalt mixture will greatly reduce its flexibility under low temperature conditions, reduce the adhesion between aggregate and asphalt, and easily cause low-temperature cracking and water damage, which will not achieve the purpose of extending the overall life of asphalt pavement. Therefore, while improving the anti-rutting performance of asphalt mixture, it is necessary to take into account its low-temperature crack resistance and water damage resistance.

[0005] At present, the commonly used high modulus agent or anti-rutting agent in my country is a mixed particle made of thermoplastic plastic as the main material. It is mixed with aggregates through dry mixing to increase the modulus of asphalt mixture, thereby improving the ability of asphalt pavement to resist permanent deformation at high temperature. However, the high modulus agent currently available on the market generally has poor compatibility with asphalt, resulting in insufficient cohesion of asphalt mixture, affecting the low temperature performance and fatigue performance of asphalt mixture. In addition, the price of high modulus agent available on the market is generally high, and there is still room for reduction.

[0006] At the same time, with the increase in the amount of asphalt pavement maintenance in my country every year, hundreds of millions of old asphalt pavement milling materials are produced every year. The asphalt in the old asphalt pavement material is asphalt that has been aged for a long time. From the macroscopic properties, the aged asphalt is characterized by an increase in softening point, a decrease in needle penetration, an increase in viscosity, and a decrease in ductility. From the microscopic properties, the components have changed, with an increase in asphaltene and colloid, a decrease in aromatic components, and a basically unchanged saturated component. From the performance of the above properties, it can be seen that the high-temperature performance of aged asphalt is significantly better than that of ordinary asphalt. Aged asphalt and aged asphalt mixtures have good high-temperature stability and strong high-temperature deformation resistance. If the aged asphalt in the old asphalt pavement is used as a basic raw material, supplemented by an efficient recycling process and compounded with other organic components, the modulus of asphalt concrete can be greatly increased, thereby improving the asphalt pavement's anti-rutting performance, low-temperature cracking performance and water damage resistance.

[0007] Based on the above reasons, a composite high modulus agent for rutting-resistant asphalt pavement is developed, which can improve the modulus of asphalt pavement and increase the anti-rutting performance without reducing the low-temperature crack resistance and water damage resistance of asphalt mixture. At the same time, it has the characteristics of low cost, green environmental protection, easy use, and easy promotion and application. Summary of the invention

[0008] In order to solve the defects of traditional asphalt pavement high modulus modifiers in the market during the promotion and application, the present invention provides a composite high modulus agent for rutting-resistant asphalt pavement and a preparation method thereof. The composite high modulus agent uses oil-rich recovered powder from the milling of old asphalt pavement as a raw material, is compounded with a variety of functional additives, and is assisted by an efficient recycling process. The modulus of the asphalt pavement can be greatly improved without reducing its low-temperature crack resistance and water damage resistance. At the same time, it is low-cost, green and environmentally friendly, easy to use, and easy to promote.

[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0010] A composite high modulus agent for rutting-resistant asphalt pavement comprises the following raw materials in parts by mass: 50%-70% recycled powder of old asphalt pavement milling material, 5%-15% composite high modulus modified asphalt, 3%-10% polyethylene wax, 2%-5% solvent oil, 5%-8% fiber, 0.1%-0.5% asphalt deodorant, and 10%-15% high molecular weight polyethylene, and the total mass meets 100%.

[0011] Preferably, the recycled powder of old asphalt pavement milling material is asphalt-rich dust generated when finely crushing and screening old asphalt pavement milling material, with a maximum particle size of less than or equal to 0.6 mm and a needle penetration of old asphalt (0.1 mm) less than or equal to 25.

[0012] Preferably, the composite high modulus modified asphalt is composed of waste tire rubber powder, SBS modifier and low-grade asphalt, the needle penetration (0.1mm) of the composite high modulus modified asphalt is less than or equal to 20, and the waste tire rubber powder accounts for 15%-20% of the total weight of the composite high modulus modified asphalt.

[0013] Preferably, the polyethylene wax has a melting point of 90°C-110°C and an average molecular weight of 3000-5000.

[0014] Preferably, the solvent oil is one of rubber oil, kerosene and diesel. The lower the viscosity of the solvent oil, the smaller the blending ratio.

[0015] Preferably, the fiber is one of basalt fiber, polypropylene fiber and glass fiber, and the fiber length is 2-5 mm.

[0016] Preferably, the particle size of the asphalt deodorizer is less than or equal to 15 μm, the dry alkali content is less than or equal to 0.2%, and the acid insoluble matter is less than or equal to 0.5%.

[0017] Preferably, the molecular weight of the high molecular weight polyethylene is not less than 100,000 and the melting point is 100-130°C.

[0018] The present invention also provides a method for preparing a composite high modulus agent for rutting-resistant asphalt pavement, the method comprising the following steps:

[0019] Step 1. Weigh according to the proportion, heat the old asphalt pavement recycled powder to 170-190℃ and put it into the reactor, then add solvent oil and force stir for 3-5 minutes;

[0020] Step 2. Add the composite high modulus modified asphalt heated to 175°C-185°C to step 1 and force stirring for 3-5 minutes;

[0021] Step 3. Add high molecular weight polyethylene, polyethylene wax and asphalt deodorizer to step 2 and force stirring for 3-5 minutes;

[0022] Step 4. Add fiber to step 3 and force stir for 5-8 minutes;

[0023] Step 5. Put the product obtained in step 4 into a granulator for extrusion granulation to obtain a composite high modulus agent.

[0024] Preferably, the temperature of the product obtained in step 4 is 80-100°C.

[0025] As a priority, the composite high modulus agent prepared according to the above steps, according to the usage amount of 0.3%-1.0% of the total weight of the asphalt mixture, the asphalt mixture performance indicators can reach: Marshall stability ≥10KN, Marshall residual stability ≥85%, freeze-thaw splitting strength ratio ≥80%, rutting test dynamic stability (60℃) ≥6000 times / mm, maximum bending tensile strain (-10℃) ≥2500με, dynamic modulus (15℃) ≥14000Mpa.

[0026] The high modulus agent for rutting-resistant asphalt pavement developed by the present invention has the following advantages:

[0027] 1. Using the recycled powder of old asphalt pavement milling material as the main raw material of the composite high modulus agent can effectively bring into play the characteristics and value of aged asphalt, recycle materials, and reduce costs;

[0028] 2. The addition of asphalt odor purifier can significantly reduce the harmful gases generated by aged asphalt, composite high modulus modified asphalt and other chemical raw materials in the production process of composite high modulus agent, and can also reduce the emission of VOC volatile organic compounds in the production process of asphalt mixture, which is beneficial to environmental protection;

[0029] 3. On the one hand, the fibers in the composite high modulus agent are beneficial to the molding and granulation of the composite high modulus agent; on the other hand, during use, the fibers are evenly distributed in the mixture in a random manner and overlap each other, forming a network entanglement structure with aggregates and asphalt binders, which greatly improves the comprehensive mechanical properties of the asphalt mixture, such as crack resistance, tensile resistance, shear resistance, compression resistance and impact resistance.

[0030] 4. High modulus composite modified asphalt has high viscosity and good adhesion with asphalt. It can effectively improve the adhesion strength between the composite high modulus agent and asphalt binder and aggregate, and improve the asphalt pavement's resistance to water damage.

[0031] 5. The addition of polyethylene wax can effectively reduce the melting point of organic compounds without reducing the performance of the composite high modulus agent, which helps to disperse the composite high modulus agent in the asphalt mixture. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic diagram of the process flow of a method for preparing a composite high modulus agent for rutting-resistant asphalt pavement according to the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0034] Example 1

[0035] A composite high modulus agent for rutting-resistant asphalt pavement comprises the following raw materials in parts by mass: 69% recycled powder of old asphalt pavement milling material, 5% composite high modulus modified asphalt, 3.9% polyethylene wax, 2% solvent oil, 5% fiber, 0.1% asphalt deodorant, and 15% high molecular weight polyethylene, and the total mass meets 100%.

[0036] Preferably, the recycled powder of old asphalt pavement milling material is asphalt-rich dust generated when finely crushing and screening old asphalt pavement milling material, with a maximum particle size of 0.6 mm and a needle penetration (0.1 mm) of 10.

[0037] Preferably, the composite high modulus modified asphalt is composed of waste tire rubber powder, SBS modifier and low-grade asphalt, the needle penetration (0.1mm) of the composite high modulus modified asphalt is 20, and the waste tire rubber powder accounts for 15% of the total weight of the composite high modulus modified asphalt.

[0038] Preferably, the polyethylene wax has a melting point of 90° C. and an average molecular weight of 3,000.

[0039] Preferably, the solvent oil is kerosene.

[0040] Preferably, the fibers are basalt fibers with a fiber length of 2 mm.

[0041] Preferably, the asphalt deodorizer has a particle size of 15 μm, a dry alkali content of 0.2%, and an acid insoluble content of 0.5%.

[0042] Preferably, the high molecular weight polyethylene has a molecular weight of 100,000 and a melting point of 130°C.

[0043] The present invention also provides a method for preparing a composite high modulus agent for rutting-resistant asphalt pavement, the method comprising the following steps:

[0044] Step 1. Weigh according to the proportion, heat the old asphalt pavement recycled powder to 190℃ and put it into the reactor, then add solvent oil and force stir for 5 minutes;

[0045] Step 2. Add the composite high modulus modified asphalt heated to 185°C to step 1 and force stirring for 3 minutes;

[0046] Step 3. Add high molecular weight polyethylene, polyethylene wax and asphalt deodorizer to step 2 and force stirring for 3 minutes;

[0047] Step 4. Add fiber to step 3 and force stir for 8 minutes;

[0048] Step 5. Put the product obtained in step 4 into a granulator for extrusion granulation to obtain a composite high modulus agent.

[0049] Preferably, the temperature of the product obtained in step 4 is 100°C.

[0050] The composite high modulus agent prepared according to the above steps, when used in an amount of 0.3% of the total weight of the asphalt mixture, can achieve the following asphalt mixture performance indicators: Marshall stability of 12KN, Marshall residual stability of 91.7%, freeze-thaw splitting strength ratio of 83%, rutting test dynamic stability (60°C) of 8190 times / mm, maximum bending tensile strain (-10°C) of 2708με, and dynamic modulus (15°C) of 15200Mpa.

[0051] Example 2

[0052] A composite high modulus agent for rutting-resistant asphalt pavement comprises the following raw materials in parts by mass: 50% recycled powder of old asphalt pavement milling material, 11.5% composite high modulus modified asphalt, 10% polyethylene wax, 5% solvent oil, 8% fiber, 0.5% asphalt deodorant, and 15% high molecular weight polyethylene, and the total mass meets 100%.

[0053] Preferably, the recycled powder of old asphalt pavement milling material is asphalt-rich dust generated when finely crushing and screening old asphalt pavement milling material, with a maximum particle size of 0.3 mm and a needle penetration (0.1 mm) of 25.

[0054] Preferably, the composite high modulus modified asphalt is composed of waste tire rubber powder, SBS modifier and low-grade asphalt, the needle penetration (0.1mm) of the composite high modulus modified asphalt is 10, and the waste tire rubber powder accounts for 20% of the total weight of the composite high modulus modified asphalt.

[0055] Preferably, the polyethylene wax has a melting point of 110° C. and an average molecular weight of 5,000.

[0056] Preferably, the solvent oil is rubber oil.

[0057] Preferably, the fibers are glass fibers with a fiber length of 5 mm.

[0058] Preferably, the asphalt deodorizer has a particle size of 10 μm, a dry alkali content of 0.1%, and an acid insoluble content of 0.22%.

[0059] Preferably, the high molecular weight polyethylene has a molecular weight of 110,000 and a melting point of 100°C.

[0060] The present invention also provides a method for preparing a composite high modulus agent for rutting-resistant asphalt pavement, the method comprising the following steps:

[0061] Step 1. Weigh according to the proportion, heat the old asphalt pavement recycled powder to 170℃ and put it into the reactor, then add solvent oil and force stir for 3 minutes;

[0062] Step 2. Add the composite high modulus modified asphalt heated to 175°C to step 1 and force stir for 5 minutes;

[0063] Step 3. Add high molecular weight polyethylene, polyethylene wax and asphalt deodorizer to step 2 and force stirring for 5 minutes;

[0064] Step 4. Add fiber to step 3 and force stir for 5 minutes;

[0065] Step 5. Put the product obtained in step 4 into a granulator for extrusion granulation to obtain a composite high modulus agent.

[0066] Preferably, the temperature of the product obtained in step 4 is 80°C.

[0067] The composite high modulus agent prepared according to the above steps, when used in an amount of 1.0% of the total weight of the asphalt mixture, can achieve the following asphalt mixture performance indicators: Marshall stability of 16KN, Marshall residual stability of 93.8%, freeze-thaw splitting strength ratio of 86%, rutting test dynamic stability (60°C) of 16000 times / mm, maximum bending tensile strain (-10°C) of 2590με, and dynamic modulus (15°C) ≥17481Mpa.

[0068] Example 3

[0069] A composite high modulus agent for rutting-resistant asphalt pavement comprises the following raw materials in parts by mass: 61% recycled powder of old asphalt pavement milling material, 15% composite high modulus modified asphalt, 4% polyethylene wax, 3.8% solvent oil, 6% fiber, 0.2% asphalt deodorant, and 10% high molecular weight polyethylene, and the total mass meets 100%.

[0070] Preferably, the recycled powder of old asphalt pavement milling material is asphalt-rich dust generated when finely crushing and screening old asphalt pavement milling material, with a maximum particle size of 0.15 mm and a needle penetration (0.1 mm) of 15 for old asphalt.

[0071] Preferably, the composite high modulus modified asphalt is composed of waste tire rubber powder, SBS modifier and low-grade asphalt. The needle penetration (0.1 mm) of the composite high modulus modified asphalt is 10, and the waste tire rubber powder accounts for 18% of the total weight of the composite high modulus modified asphalt.

[0072] Preferably, the polyethylene wax has a melting point of 100° C. and an average molecular weight of 4,000.

[0073] Preferably, the solvent oil is diesel.

[0074] Preferably, the fibers are polypropylene fibers with a fiber length of 3 mm.

[0075] The preferred asphalt deodorizer has a particle size of 9 μm, a dry alkali content of 0.05%, and an acid insoluble content of 0.1%.

[0076] Preferably, the high molecular weight polyethylene has a molecular weight of 200,000 and a melting point of 121°C.

[0077] The present invention also provides a method for preparing a composite high modulus agent for rutting-resistant asphalt pavement, the method comprising the following steps:

[0078] Step 1. Weigh according to the proportion, heat the old asphalt pavement recycled powder to 175℃ and put it into the reactor, then add solvent oil and force stir for 4 minutes;

[0079] Step 2. Add the composite high modulus modified asphalt heated to 180°C to step 1 and force stirring for 4 minutes;

[0080] Step 3. Add high molecular weight polyethylene, polyethylene wax and asphalt deodorizer to step 2 and force stirring for 4 minutes;

[0081] Step 4. Add fiber to step 3 and force stir for 6 minutes;

[0082] Step 5. Put the product obtained in step 4 into a granulator for extrusion granulation to obtain a composite high modulus agent.

[0083] Preferably, the temperature of the product obtained in step 4 is 90°C.

[0084] The composite high modulus agent prepared according to the above steps, when used in an amount of 0.4% of the total weight of the asphalt mixture, can achieve the following asphalt mixture performance indicators: Marshall stability of 13.5KN, Marshall residual stability of 93.9, freeze-thaw splitting strength ratio of 89.1%, rutting test dynamic stability (60°C) of 12619 times / mm, maximum bending tensile strain (-10°C) of 2611με, and dynamic modulus (15°C) of 15766Mpa.

[0085] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A composite high modulus agent for anti-rutting asphalt pavement, characterized in that: It contains the following raw materials in parts by mass: 50%-70% recycled powder of old asphalt pavement milling materials, 5%-15% composite high modulus modified asphalt, 3%-10% polyethylene wax, 2%-5% solvent oil, 5%-8% fiber, 0.1%-0.5% asphalt deodorizer, and 10%-15% high molecular weight polyethylene, and the total mass meets 100%. Preferably, the recycled powder of old asphalt pavement milling material is asphalt-rich dust generated when finely crushing and screening old asphalt pavement milling material, with a maximum particle size of less than or equal to 0.6 mm and a needle penetration of old asphalt (0.1 mm) less than or equal to 25. Preferably, the composite high modulus modified asphalt is composed of waste tire rubber powder, SBS modifier and low-grade asphalt, the needle penetration (0.1mm) of the composite high modulus modified asphalt is less than or equal to 20, and the waste tire rubber powder accounts for 15%-20% of the total weight of the composite high modulus modified asphalt. Preferably, the solvent oil is one of rubber oil, kerosene and diesel. The lower the viscosity of the solvent oil, the smaller the blending ratio. Preferably, the fiber is one of basalt fiber, polypropylene fiber and glass fiber, and the fiber length is 2-5 mm. Preferably, the particle size of the asphalt deodorizer is less than or equal to 15 μm, the dry alkali content is less than or equal to 0.2%, and the acid insoluble matter is less than or equal to 0.5%.

2. The method for preparing a composite high modulus agent for rutting-resistant asphalt pavement according to claim 1, characterized in that: The method comprises the following steps: Step 1. Weigh according to the proportion, heat the old asphalt pavement recycled powder to 170-190℃ and put it into the reactor, then add solvent oil and force stir for 3-5 minutes; Step 2. Add the composite high modulus modified asphalt heated to 175°C-185°C to step 1 and force stirring for 3-5 minutes; Step 3. Add high molecular weight polyethylene, polyethylene wax and asphalt deodorizer to step 2 and force stirring for 3-5 minutes; Step 4. Add fiber to step 3 and force stir for 5-8 minutes; Step 5. Put the product obtained in step 4 into a granulator for extrusion granulation to obtain a composite high modulus agent.

Citation Information

Cited By

  • Full-RAP cold-recycled asphalt mixture based on trace new asphalt and preparation method of full-RAP cold-recycled asphalt mixture