Fluidic foam geopolymer filling material and preparation method thereof

By adding reduced graphene oxide and alkali-excited metakaolin to the geopolymer foam concrete, a fluid foam geopolymer filling material is formed, which solves the problems of uneven pore structure and low compressive strength, and significantly improves the durability of the material and adaptability, and reduce carbon dioxide emissions.

CN118908633APending Publication Date: 2024-11-08HUNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410952210.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing poly foam concrete materials have problems such as uneven pore structure, low compressive strength and poor durability, which are difficult to meet the needs of building materials in extreme climates.

Method used

Using a fluid foamed polymer filling material, including powders, alkali triggers, reduced graphene oxide, hydrogen peroxide and sodium stearate, the structure is enhanced, interface bonding is improved, and the microscopic is improved by incorporating reduced graphene oxide. Structural and thermal stability, combined with alkali, stimulates the gelation reaction of metakaolin to reduce carbon dioxide emissions.

Benefits of technology

It significantly improves the compressive flexural strength and durability of the geopolymer foam filling material, adapts to high temperature and cold environments, reduces carbon dioxide emissions, and improves the reliability and adaptability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908633A_ABST
    Figure CN118908633A_ABST
Patent Text Reader

Abstract

The invention discloses a flow-state foam geopolymer filling material and a preparation method thereof, and belongs to the technical field of building materials. The flow-state foam geopolymer filling material comprises powder, an alkali activator, water, reduced graphene oxide, hydrogen peroxide and sodium stearate, the alkali activator accounts for 15% of the mass of the powder, the water accounts for 10% of the mass of the powder, the reduced graphene oxide accounts for 0.03%-0.15% of the mass of the powder, the hydrogen peroxide accounts for 1.5% of the mass of the powder, and the powder comprises, by weight, 80-90 parts of tile slate tailings and 10-20 parts of metakaolin. The geopolymer foam filling material has the beneficial effects that by doping the reduced graphene oxide (rGO), the pore structure of the geopolymer foam filling material is effectively improved, various properties of the geopolymer foam filling material are improved, and compared with the traditional method, the emission of carbon dioxide can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a fluid foam geopolymer filling material and a preparation method thereof. Background Art

[0002] Existing research results show that the geopolymer foam concrete materials currently produced generally have performance problems such as uneven pore structure and low compressive strength. Affected by extreme climate, building materials are facing increasingly harsh environmental conditions, and the requirements for the durability of building materials have become higher. However, the durability of existing geopolymer foam concrete materials is poor and it is difficult to meet the actual engineering needs. Therefore, it is urgent to improve the formula of foam filling materials to improve their pore structure, mechanical properties and durability. Summary of the invention

[0003] The object of the present invention is to provide a fluid foam geopolymer filling material and a preparation method thereof, which can solve at least one technical problem involved in the background technology.

[0004] In order to solve the above-mentioned technical problems, the present invention is achieved as follows:

[0005] The invention provides a fluidized foam geopolymer filling material, comprising powder and 15% of the weight of the powder respectively of an alkali activator, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80-90 parts of slate tailings and 10-20 parts of metakaolin by weight.

[0006] Optionally, the alkaline activator is prepared by adding 8 parts of analytically pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving the solution.

[0007] Optionally, it includes powder and 15% of the mass of the powder respectively consisting of an alkali activator, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80-90 parts of slate tailings and 10-20 parts of kaolin by weight.

[0008] Optionally, it includes powder and 15% of the mass of the powder respectively consisting of an alkali activator, 10% of water, 0.03% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder includes 85 parts of slate tailings and 15 parts of kaolin by weight.

[0009] Optionally, it includes powder and 15% of the mass of the powder respectively consisting of an alkali activator, 10% of water, 0.03% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder includes 80 parts of slate tailings and 20 parts of kaolin by weight.

[0010] Optionally, it includes powder and 15% of the mass of the powder respectively constituted by an alkali activator, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 85 parts of slate tailings and 15 parts of kaolin by weight.

[0011] Optionally, it includes powder and 15% of the mass of the powder respectively consisting of an alkali activator, 10% of water, 0.06% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 85 parts of slate tailings and 15 parts of kaolin by weight.

[0012] Optionally, it includes powder and 15% of the mass of the powder respectively consisting of an alkali activator, 10% of water, 0.09% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder includes 85 parts of slate tailings and 15 parts of kaolin by weight.

[0013] Optionally, it includes powder and 15% of the mass of the powder respectively consisting of an alkali activator, 10% of water, 0.12% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 85 parts of slate tailings and 15 parts of kaolin by weight.

[0014] The present invention also provides a method for preparing the fluid foam geopolymer filling material, which comprises the following steps:

[0015] Step 1, providing a powder and an alkali activator accounting for 15% of the weight of the powder, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80-90 parts of slate tailings and 10-20 parts of metakaolin by weight;

[0016] Step 2, mix the powder evenly;

[0017] Step 3, mixing the alkaline activator, water and reduced graphene oxide evenly, adding the mixture to the evenly mixed powder and continuing to stir evenly to obtain a mixture A;

[0018] Step 4, adding sodium stearate to mixture A and stirring evenly to obtain mixture B;

[0019] Step 5, adding hydrogen peroxide to mixture B and stirring evenly to obtain mixture C;

[0020] Step six, pouring the mixture C into a mold for molding, demoulding after 1 day, and curing under constant temperature and humidity conditions for 7 days to obtain a fluidized foamed geopolymer filling material.

[0021] The beneficial effects of the present invention are as follows:

[0022] 1. By incorporating reduced graphene oxide (rGO), multiple mechanisms such as structural reinforcement, interface bonding, microstructure modification, and enhanced thermal stability and low-temperature toughness are achieved, which significantly improves the compressive and flexural strength of geopolymer foam filling materials and their performance in extreme environments such as high temperature and cold, making geopolymer foam filling materials more adaptable and more reliable in construction and engineering applications;

[0023] 2. By adding reduced graphene oxide (rGO), the pore structure of the geopolymer foam filling material is effectively improved, the various properties of the geopolymer foam filling material are increased, and compared with traditional methods, carbon dioxide emissions can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:

[0025] Figure 1 This is a particle grading diagram of slate tailings provided by the present invention. DETAILED DESCRIPTION

[0026] The technical solutions in the present invention will be described clearly and completely below in combination with the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The present invention provides a fluidized foam geopolymer filling material, comprising powder and 15% of the mass of the powder respectively of an alkali activator, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80-90 parts of slate tailings and 10-20 parts of metakaolin by weight.

[0028] The alkaline activator is prepared by adding 8 parts of analytically pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and then completely dissolving the solution.

[0029] It should be noted that the metakaolin, slate tailings and reduced graphene oxide are gelled under the action of an alkali activator, hydrogen peroxide and sodium stearate. The fluid foam geopolymer filling material provided by the present invention utilizes slate tailings and uses an alkali activator to activate the metakaolin. There is no CO in the production process. 2 Emissions, and the various properties of geopolymer foam concrete are enhanced by reducing graphene oxide, making it have excellent durability, high added value, and in line with the needs of low-carbon development. It is of great significance for the resource reuse of slate tailings, the performance improvement of geopolymer foam filling materials and the reduction of carbon dioxide emissions in the construction industry.

[0030] In the prior art, the use of tailings supplemented with cement and foaming agent to prepare tailings foam concrete will emit a large amount of carbon dioxide (see Table 1 below), and the tailings foam concrete has low compressive and flexural strength, poor durability, and high cost. The present invention reduces the emission of carbon dioxide by alkali-activated metakaolin, and has high compressive and flexural strength. At the same time, the addition of reduced graphene oxide enhances the strength and durability of the slate tailings-metakaolin polymer foam filling material, thereby enhancing the availability of the slate tailings-metakaolin polymer foam filling material, reducing the accumulation of tailings and solving environmental problems, and preparing a slate tailings-metakaolin polymer foam filling material with excellent performance, which has great economic significance.

[0031] Table 1 Carbon dioxide emissions from common tailings foam concrete

[0032]

[0033]

[0034] The tile slate particles of the present invention are relatively small, and the SiO 2 、Al 2 O 3 This makes it have a certain activity, so that part of the slate also participates in the alkali excitation reaction, further increasing the compressive and flexural strength of the slate-metakaolin polymer foam filling material. The chemical composition of the slate tailings and mineral powder used in the present invention is shown in Table 2.

[0035] Table 2 Main chemical components of slate tailings and metakaolin used in the present invention

[0036] raw materials <![CDATA[SiO 2 ]]> <![CDATA[ 2 THE 3 ]]> <![CDATA[Fe 2 THE 3 ]]> CaO MgO <![CDATA[Na 2 The]]> tile slate tailings 42.17 9.15 9.02 30.37 5.16 0.53 Metakaolin 54.25 43.19 1.03 0.23 0.66 0.28

[0037] The slate tailings used in the present invention come from the slate tailings after mining a mine in a tailings pond in Langao County, Shaanxi Province. Figure 1 As shown, it can be seen that its particle size is small, so it has a certain activity. The metakaolin used in the present invention is a white powder. The alkaline activator in the present invention is prepared by mixing sodium silicate solution with analytical pure sodium hydroxide. The modulus of the sodium silicate solution in the present invention is 2.31, the content is 42%, and the Baume degree is 50. The analytical pure NaOH used is in powder form with a purity of ≥96%. Hydrogen peroxide (H 2 O 2 ), with a mass fraction of 30%. Use analytically pure standard sodium stearate. The molecular formula of sodium stearate is C 18 H 35 NaO 2 , molecular weight is 306.46.

[0038] Furthermore, the present invention can significantly enhance the compressive and flexural strength and the performance of extreme environments such as high temperature and cold resistance by adding reduced graphene oxide (rGO) into the geopolymer foam filling material, and the mechanism is as follows:

[0039] Nano-reinforcement: Reduced graphene oxide (rGO) is a two-dimensional nanomaterial with high strength and high modulus. After incorporation of rGO, these nanosheets form a nano-reinforced network in the geopolymer matrix, which can effectively improve the overall strength and stiffness of the material.

[0040] Load transfer: The rGO sheets are evenly dispersed in the geopolymer matrix, which can effectively transfer and disperse stress when subjected to external forces, reduce stress concentration, and thus improve compressive and flexural strength.

[0041] Interfacial interactions: rGO has a large number of oxidized groups, which can form strong chemical bonds or hydrogen bonds with the aluminosilicates in the geopolymer matrix, enhancing the interfacial bonding and improving the overall strength of the material.

[0042] Surface effect: The high specific surface area of ​​rGO provides more interface areas, making the interface bonding between the geopolymer matrix and rGO closer, thereby improving the mechanical properties of the material.

[0043] Micropore filling: rGO can fill the tiny pores in the geopolymer matrix, reducing the porosity and thus increasing the density and strength of the material.

[0044] Lattice defect repair: rGO can repair lattice defects in the geopolymer matrix, reduce the generation and expansion of microcracks, and thus improve the flexural and compressive strength of the material.

[0045] Thermal stability: rGO has excellent thermal stability and high melting point, and can remain stable in high temperature environments. After adding rGO, the thermal stability and high temperature resistance of geopolymer materials are significantly improved.

[0046] Thermal conduction: rGO's high thermal conductivity can quickly conduct and disperse heat, reduce the damage of local high temperature to the material, and further enhance the material's high temperature resistance.

[0047] Low-temperature toughness: rGO can maintain good toughness at low temperatures. After adding rGO, the brittleness of geopolymer materials in cold environments is reduced and the toughness is enhanced, thereby improving the cold resistance of the material.

[0048] Thermal expansion matching: The thermal expansion coefficients of rGO and the geopolymer matrix are matched, reducing thermal stress caused by temperature changes, thereby improving the cold resistance of the material.

[0049] In summary, the incorporation of reduced graphene oxide (rGO) significantly improves the compressive and flexural strength of geopolymer foam filling materials and their performance in extreme environments such as high temperature and cold through multiple mechanisms such as structural reinforcement, interface bonding, microstructure modification, and enhanced thermal stability and low-temperature toughness. This makes geopolymer foam filling materials more widely adaptable and more reliable in construction and engineering applications.

[0050] The present invention also provides a method for preparing the fluid foam geopolymer filling material, which comprises the following steps:

[0051] Step 1, providing a powder and an alkali activator accounting for 15% of the weight of the powder, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80-90 parts of slate tailings and 10-20 parts of metakaolin by weight;

[0052] Step 2, mix the powder evenly;

[0053] Step 3, mixing the alkaline activator, water and reduced graphene oxide evenly, adding the mixture to the evenly mixed powder and continuing to stir evenly to obtain a mixture A;

[0054] Step 4, adding sodium stearate to mixture A and stirring evenly to obtain mixture B;

[0055] Step 5, adding hydrogen peroxide to mixture B and stirring evenly to obtain mixture C;

[0056] Step six, pouring the mixture C into a mold for molding, demoulding after 1 day, and curing under constant temperature and humidity conditions for 7 days to obtain a fluidized foamed geopolymer filling material.

[0057] The fluidized foam geopolymer filling material and the preparation method thereof provided by the present invention are described in detail with reference to specific examples 1-7.

[0058] Example 1

[0059] In this embodiment, the fluidized foam geopolymer filling material is composed of powder, alkaline activator, water, reduced graphene oxide, hydrogen peroxide and sodium stearate, wherein the powder component is a mixture of 90 parts of slate tailings and 10 parts of kaolin; the alkaline activator in this embodiment is prepared by adding 8 parts of analytical pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving them.

[0060] In this embodiment, after the powders are mixed evenly, 15% of the mass of the powders' alkali activator, 10% of water and 0.03% of reduced graphene oxide are mixed evenly and added to the powders. After stirring evenly, 0.4% of sodium stearate is added and stirred evenly, and then 1.5% of hydrogen peroxide is added. After forming, the mixture is poured into a mold and molded. After one day, the mixture is demolded and cured at a constant temperature and humidity for 7 days.

[0061] Example 2

[0062] In this embodiment, the fluidized foam geopolymer filling material is composed of powder, alkali activator and water, wherein the powder component is a mixture of 85 parts of slate tailings and 15 parts of kaolin; the alkali activator in this embodiment is prepared by adding 8 parts of analytical pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving them.

[0063] The preparation steps are the same as those in Example 1.

[0064] Example 3

[0065] In this embodiment, the fluidized foam geopolymer filling material is composed of powder, alkali activator and water, wherein the powder component is a mixture of 80 parts of slate tailings and 20 parts of kaolin; the alkali activator in this embodiment is prepared by adding 8 parts of analytical pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving them.

[0066] The preparation steps are the same as those in Example 1.

[0067] Example 4

[0068] In this embodiment, the fluidized foam geopolymer filling material is composed of powder, alkali activator and water, wherein the powder component is a mixture of 85 parts of slate tailings and 15 parts of kaolin; the alkali activator in this embodiment is prepared by adding 8 parts of analytical pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving them.

[0069] In this embodiment, after the powders are mixed evenly, 15% of the powder mass of the alkali activator, 10% of the water and 0.06% of the reduced graphene oxide are mixed evenly and added to the powders. After stirring evenly, 0.4% of sodium stearate is added and stirred evenly, and then 1.5% of hydrogen peroxide is added. After molding, the mixture is poured into a mold, molded after 1 day, and cured under constant temperature and humidity conditions for 7 days.

[0070] Example 5

[0071] In this embodiment, the fluidized foam geopolymer filling material is composed of powder, alkali activator and water, wherein the powder component is a mixture of 85 parts of slate tailings and 15 parts of kaolin; the alkali activator in this embodiment is prepared by adding 8 parts of analytical pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving them.

[0072] In this embodiment, after the powders are mixed evenly, 15% of the powder mass of the alkali activator, 10% of the water and 0.09% of the reduced graphene oxide are mixed evenly and added to the powders. After stirring evenly, 0.4% of sodium stearate is added and stirred evenly, and then 1.5% of hydrogen peroxide is added. After molding, the mixture is poured into a mold, demolded after 1 day, and cured under constant temperature and humidity conditions for 7 days.

[0073] Example 6

[0074] In this embodiment, the fluidized foam geopolymer filling material is composed of powder, alkali activator and water, wherein the powder component is a mixture of 85 parts of slate tailings and 15 parts of kaolin; the alkali activator in this embodiment is prepared by adding 8 parts of analytical pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving them.

[0075] In this embodiment, after the powders are mixed evenly, 15% of the powder mass of the alkali activator, 10% of the water and 0.12% of the reduced graphene oxide are mixed evenly and added to the powders. After stirring evenly, 0.4% of sodium stearate is added and stirred evenly, and then 1.5% of hydrogen peroxide is added. After molding, the mixture is poured into a mold, molded after 1 day, and cured under constant temperature and humidity conditions for 7 days.

[0076] Example 7

[0077] In this embodiment, the fluidized foam geopolymer filling material is composed of powder, alkali activator and water, wherein the powder component is a mixture of 85 parts of slate tailings and 15 parts of kaolin; the alkali activator in this embodiment is prepared by adding 8 parts of analytical pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving them.

[0078] In this embodiment, after the powders are mixed evenly, 15% of the powder mass of an alkali activator, 10% of water and 0.15% of reduced graphene oxide are mixed evenly and added to the powders. After stirring evenly, the mixture is poured into a special mold for molding, and the mixture is demolded after 1 day and cured under constant temperature and humidity conditions for 7 days.

[0079] Comparative Example

[0080] In this comparative example, the fluidized foam geopolymer filling material is composed of powder, alkali activator and water, wherein the powder component is a mixture of 85 parts of slate tailings and 15 parts of kaolin; the alkali activator in this implementation case is prepared by adding 8 parts of analytical pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and completely dissolving them.

[0081] In this embodiment, after the powders are mixed evenly, 15% of the powder mass of an alkali activator and 10% of water are mixed evenly and added to the powders. After stirring evenly, the mixture is poured into a special mold for molding. The mixture is demoulded after 1 day and cured under constant temperature and humidity conditions for 7 days.

[0082] After preparing the above cases, we measured their performance parameters and the results are shown in the following table:

[0083] Table 3 Test results

[0084]

[0085]

[0086] It can be seen from the test results in Table 3 that the compressive and flexural strengths of the reduced graphene oxide enhanced kaolin-slate tailings geopolymer foam filling materials of Examples 1-7 of the present invention are improved compared with the comparative example, and the addition of reduced graphene oxide significantly increases the flexural strength of the geopolymer foam filling material. Compared with the comparative example, the flexural strength of Example 7 is increased by 67.7%. It is explained that the geopolymer foam filling material prepared by using kaolin-iron tailings of the present invention has good strength, can replace or partially replace foam concrete in the construction industry, and it can be observed that with the increase of the amount of reduced graphene oxide added, its porosity decreases. Compared with the comparative example, the porosity of Example 7 is reduced from 48.31 to 45.21, which shows that the addition of reduced graphene oxide improves the pore structure of the geopolymer foam filling material, thereby enhancing its strength and durability. Specifically, compared with the comparative example, the freeze-thaw cycle strength loss rate of Example 7 is reduced from 52.26% to 37.90%, and the strength loss rate after calcination is reduced from 50.5% to 30.2%.

[0087] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0088] In addition, it should be noted that the scope of the methods and preparation methods in the embodiments of the present invention is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved. For example, the described methods may be performed in an order different from that described, and various steps may be added, omitted, or combined. In addition, features described with reference to certain examples may be combined in other examples.

[0089] The embodiments of the present invention are described above, but the present invention is not limited to the above-mentioned specific implementation modes. The above-mentioned specific implementation modes are merely illustrative and not restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the purpose of the present invention and the claims, all of which are protected by the present invention.

Claims

1. A fluid foam geopolymer filling material, characterized in that: The invention comprises powder and 15% of the weight of the powder respectively of an alkali activator, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80-90 parts of slate tailings and 10-20 parts of metakaolin by weight.

2. The fluid foam geopolymer filling material according to claim 1, characterized in that: The alkaline activator is prepared by adding 8 parts of analytically pure sodium hydroxide to 100 parts of sodium silicate solution at room temperature and then completely dissolving the solution.

3. The fluid foam geopolymer filling material according to claim 1 or 2, characterized in that: The invention comprises powder and 15% of the weight of the powder respectively of an alkali activator, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80-90 parts of slate tailings and 10-20 parts of metakaolin by weight.

4. The fluid foam geopolymer filling material according to claim 1 or 2, characterized in that: The invention comprises powder and 15% of the weight of the powder respectively of an alkali activator, 10% of water, 0.03% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 85 parts of slate tailings and 15 parts of metakaolin.

5. The fluid foam geopolymer filling material according to claim 1 or 2, characterized in that: The invention comprises powder and 15% of the mass of the powder respectively of an alkali activator, 10% of water, 0.03% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80 parts of slate tailings and 20 parts of metakaolin by weight.

6. The fluid foam geopolymer filling material according to claim 1 or 2, characterized in that: The invention comprises powder and 15% of the weight of the powder respectively of an alkali activator, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 85 parts of slate tailings and 15 parts of metakaolin by weight.

7. The fluid foam geopolymer filling material according to claim 1 or 2, characterized in that: The invention comprises powder and 15% of the weight of the powder respectively of an alkali activator, 10% of water, 0.06% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 85 parts of slate tailings and 15 parts of metakaolin by weight.

8. The fluid foam geopolymer filling material according to claim 1 or 2, characterized in that: The invention comprises powder and 15% of the mass of the powder respectively of an alkali activator, 10% of water, 0.09% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 85 parts of slate tailings and 15 parts of metakaolin by weight.

9. The fluid foam geopolymer filling material according to claim 1 or 2, characterized in that: The invention comprises powder and 15% of the weight of the powder respectively of an alkali activator, 10% of water, 0.12% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 85 parts of slate tailings and 15 parts of metakaolin.

10. A method for preparing a fluid foam geopolymer filling material according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: Step 1, providing a powder and an alkali activator accounting for 15% of the weight of the powder, 10% of water, 0.03%-0.15% of reduced graphene oxide, 1.5% of hydrogen peroxide and 0.4% of sodium stearate, wherein the powder comprises 80-90 parts of slate tailings and 10-20 parts of metakaolin by weight; Step 2, mix the powder evenly; Step 3, mixing the alkaline activator, water and reduced graphene oxide evenly, adding the mixture to the evenly mixed powder and continuing to stir evenly to obtain a mixture A; Step 4, adding sodium stearate to mixture A and stirring evenly to obtain mixture B; Step 5, adding hydrogen peroxide to mixture B and stirring evenly to obtain mixture C; Step six, pouring the mixture C into a mold for molding, demoulding after 1 day, and curing under constant temperature and humidity conditions for 7 days to obtain a fluidized foamed geopolymer filling material.