Lepidolite particle insulating brick and preparation method thereof

Through the preparation and cement combination of lithium mica particles, the problems of low consumption of lithium mica leaching slag and complex process are solved, and efficient production of lithium mica insulation bricks is achieved, which improves thermal insulation performance and compressive strength, which is suitable for large-scale industrialization Apply and reduce environmental pollution.

CN118908642AActive Publication Date: 2024-11-08HUNAN ZIJIN LITHIUM POLYMETALLIC NEW MATERIALS CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410747279.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-11-08
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

In the prior art, the consumption of lithium mica leaching slag is low, difficult to absorb on a large scale, and the preparation process is complex and costly, resulting in poor insulation effect of lithium mica slag, low compressive strength, and adversely affecting the environment.

Method used

Lithium mica particles are used as raw materials and are combined with cement after granulation, roasting and leaching to prepare lithium mica insulation bricks with light weight, high compressive strength and excellent insulation performance, simplifying the process flow and reducing production energy consumption.

Benefits of technology

Large-scale absorption of lithium mica particles has been achieved, the insulation performance and compressive strength have been improved, production costs have been reduced, suitable for industrial applications, and environmental pollution has been reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908642A_ABST
    Figure CN118908642A_ABST
Patent Text Reader

Abstract

The invention discloses a lepidolite particle insulating brick and a preparation method thereof, the lepidolite particle insulating brick is prepared from the following raw materials in percentage by mass: 40-80% of lepidolite particles and 20-60% of cement, and the lepidolite particles are prepared by taking lepidolite as a raw material through granulation, roasting and leaching. In the invention, the lepidolite particles have the characteristics of low density, high porosity, low heat conductivity coefficient, high strength and the like, and the lepidolite particle insulating brick with light weight, high compressive strength and excellent thermal insulation performance can be formed after the lepidolite particles are compounded with the cement; the adopted lepidolite particles can be directly utilized and do not need to be subjected to pretreatment such as grinding and drying, the preparation process is simpler, operation is more convenient, production energy consumption is lower, the preparation method is suitable for large-scale preparation, industrial application of the lepidolite particle insulating brick is convenient to achieve, the adopted lepidolite particles are large in dosage, and the cost is low. The method can realize large-quantity resource utilization of the lepidolite particles, and can effectively solve the environmental problem of the lepidolite particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials and relates to a lithium mica particle insulation brick and a preparation method thereof. Background Art

[0002] Lepidolite is an important raw material for the smelting and production of lithium carbonate. In the process of using lepidolite to smelt lithium carbonate, a large amount of leaching residue will be produced. These lepidolite leaching residues are both a usable resource and a pollutant. Therefore, obtaining an effective disposal method for lepidolite leaching residues is a major problem faced at the current stage.

[0003] At present, the main disposal method adopted by the industry is to store the lithium mica leaching slag in a tailings disposal site, which has the following defects: it requires a large amount of land and has high construction costs; the stockpile volume is large, the operation and maintenance pressure is high, and the cost is high; it may damage the local ecological environment.

[0004] In response to the above problems, researchers have proposed strategies to use lithium mica leaching residue as raw materials in the construction industry. There are two main strategies: one is to use lithium mica leaching residue as raw material to make composite gel materials, for example, lithium slag, silicate cement, silica ash and other materials are mixed and ground to obtain composite gelling materials; or, powdered lithium slag is mixed with fly ash, activator, water reducer, chelating agent, water, and curing to obtain lithium slag geopolymer materials; for example, lithium mica slag is used as cement admixture to prepare silicate cement. The second is to use lithium mica leaching residue as raw material to make building bricks, for example, lithium mica leaching residue is used as raw material, mixed with construction waste, ceramic waste and other materials, sintered, and ceramic bricks are obtained. The above treatment methods still have the following defects: high energy consumption, low consumption of lithium mica leaching residue, and it is difficult to consume lithium mica leaching residue on a large scale. In addition, in order to increase the consumption of lithium mica slag, some researchers have proposed a method for preparing calcium silicate board using lithium mica slag, wherein lithium mica slag, cement and pulp are used as raw materials to make slurry, and then the slurry is formed, pre-cured and autoclaved to make calcium silicate board. However, this method still has the following defects: (1) The lithium mica slag used is lithium mica and sulfate as raw materials, and is prepared by mixing, roasting, water immersion and solid-liquid separation. The lithium mica slag is a fine powder with low porosity, high density, high thermal conductivity and low strength. When used to prepare calcium silicate board, it is not conducive to improving the compressive strength and does not have a good thermal insulation effect. The thermal insulation effect is poor. Furthermore, although By adding pulp, the bending strength can be improved and the density can be reduced, but it is still difficult to effectively improve the compressive strength and reduce the weight of the calcium silicate board. In particular, it is difficult to effectively reduce the thermal conductivity, which is not conducive to improving the thermal insulation effect. In addition, adding a large amount of pulp will inevitably reduce the consumption of lithium mica slag and increase the production cost; (2) Before using the lithium mica slag, the lithium mica slag needs to be skipped and screened, and the slurry needs to be autoclaved and cured, which makes the preparation process still have the defects of complex process, inconvenient operation, harsh preparation conditions, high preparation cost, low preparation efficiency, etc., and it is difficult to quickly consume large-scale lithium mica slag, which is not conducive to the industrial application of lithium mica slag. Therefore, obtaining a lithium mica slag with low density, high porosity, low thermal conductivity and high strength, and making it into a light, high compressive strength and excellent thermal insulation brick is of great significance for large-scale consumption of lithium mica slag and harmless treatment and resource utilization of lithium mica slag. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a lithium mica particle insulation brick with light weight, high compressive strength and excellent thermal insulation performance and a preparation method thereof in view of the above-mentioned problems in the prior art.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0007] A lepidolite thermal insulation brick, wherein the lepidolite thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0008] Lepidolite particles 40% to 80%,

[0009] Cement 20%~60%;

[0010] The lepidolite particles are prepared by using lepidolite as a raw material through granulation, roasting and leaching.

[0011] The above-mentioned lithium mica particle insulation brick is further improved, and the preparation method of the lithium mica particle comprises the following steps:

[0012] S1, mixing lepidolite concentrate, a roasting additive and a volatile binder to obtain a mixture B;

[0013] S2, finely grinding the mixture B until the particle size is above 200 meshes to obtain the mixture C;

[0014] S3, mixing mixed material C with water to obtain mixed material D;

[0015] S4, granulating the mixed material D to obtain lepidolite concentrate particles;

[0016] S5, roasting the lithium ore concentrate particles;

[0017] S6. Leaching the product obtained after roasting, separating the solid from the liquid, and obtaining lithium mica particles.

[0018] The above-mentioned lithium mica thermal insulation brick is further improved. In step S1, the mass ratio of the lithium mica concentrate to the roasting additive is 1:0.1-0.8; the added amount of the volatile binder is 1%-10% of the total mass of the lithium mica concentrate and the roasting additive; the roasting additive is at least one of calcium sulfate, calcium carbonate, sodium sulfate and potassium sulfate or a mixture thereof; the mass percentage of lithium in the lithium ore concentrate is ≥1.5%; the volatile binder is at least one of semi-coke and petroleum coke.

[0019] The above-mentioned lithium mica thermal insulation brick is further improved, in step S2, the particle size of the mixture C is 300 mesh to 1000 mesh.

[0020] The above-mentioned lithium mica thermal insulation brick is further improved, in step S3, the amount of water added is 5% to 20% of the total mass of the mixture C.

[0021] The above-mentioned lepidolite thermal insulation brick is further improved, in step S4, the particle size of the lepidolite concentrate particles is 8mm to 10mm.

[0022] The above-mentioned lithium mica particle insulation brick is further improved. In step S5, a rotary kiln is used to roast the lithium ore concentrate particles; the roasting temperature is 850° C. to 900° C.; and the roasting time is 30 min to 50 min.

[0023] The above-mentioned lithium mica thermal insulation brick is further improved. In step S6, the product obtained after roasting is placed in water for leaching; the liquid-solid ratio is controlled to be 0.8-1:1 during the leaching process; and the leaching time is 3 to 4 days.

[0024] The above-mentioned lithium mica thermal insulation brick is further improved, and the lithium mica thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0025] Lepidolite particles 60% to 80%,

[0026] Cement 20%~40%.

[0027] The above-mentioned lithium mica thermal insulation brick is further improved in that the particle size of the lithium mica particles is distributed between 5mm and 10mm; and the cement is at least one of composite silicate cement, slag silicate cement, fly ash silicate cement, and ferroaluminate cement.

[0028] As a general technical concept, the present invention also provides a method for preparing a lepidolite particle insulation brick, comprising the following steps:

[0029] (1) Mixing cement and water and stirring to obtain slurry;

[0030] (2) adding lithium mica particles to the slurry and stirring to obtain a mixture; the lithium mica particles are prepared by granulating, roasting and leaching lithium mica as a raw material;

[0031] (3) The mixture is pressed into shape and cured to obtain lithium mica thermal insulation bricks.

[0032] The preparation method of the above-mentioned lithium mica particle insulation brick is further improved. In step (1), the amount of water added is 15% to 20% of the mass of cement; and the cement is at least one of composite silicate cement, slag silicate cement, fly ash silicate cement, and ferroaluminate cement.

[0033] The method for preparing the above-mentioned lithium mica thermal insulation brick is further improved, in which in step (2), the mass ratio of lithium mica particles to cement in the mixture is 2-4:1-3; and the particle size distribution of the lithium mica particles is between 5mm and 10mm.

[0034] The above-mentioned method for preparing the lepidolite thermal insulation brick is further improved, in step (2), the method for preparing the lepidolite particles comprises the following steps:

[0035] S1, mixing lepidolite concentrate, a roasting additive and a volatile binder to obtain a mixture B;

[0036] S2, finely grinding the mixture B until the particle size is above 200 meshes to obtain the mixture C;

[0037] S3, mixing mixed material C with water to obtain mixed material D;

[0038] S4, granulating the mixed material D to obtain lepidolite concentrate particles;

[0039] S5, roasting the lithium ore concentrate particles;

[0040] S6. Leaching the product obtained after roasting, separating the solid from the liquid, and obtaining lithium mica particles.

[0041] The preparation method of the above-mentioned lithium mica particle insulation brick is further improved. In step S1, the mass ratio of the lithium mica concentrate to the roasting additive is 1:0.1-0.8; the added amount of the volatile binder is 1%-10% of the total mass of the lithium mica concentrate and the roasting additive; the roasting additive is at least one of calcium sulfate, calcium carbonate, sodium sulfate and potassium sulfate or a mixture thereof; the mass percentage of lithium in the lithium ore concentrate is ≥1.5%; the volatile binder is at least one of semi-coke and petroleum coke.

[0042] The above-mentioned method for preparing the lepidolite thermal insulation brick is further improved, in which in step S2, the particle size of the mixture C is 300 mesh to 1000 mesh.

[0043] The above-mentioned method for preparing the lepidolite thermal insulation brick is further improved, in which in step S3, the amount of water added is 5% to 20% of the total mass of the mixture C.

[0044] The method for preparing the above-mentioned lepidolite thermal insulation brick is further improved, in which in step S4, the particle size of the lepidolite concentrate particles is 8 mm to 10 mm.

[0045] The method for preparing the above-mentioned lithium mica particle insulation brick is further improved. In step S5, a rotary kiln is used to roast the lithium ore concentrate particles; the roasting temperature is 850° C. to 900° C.; and the roasting time is 30 min to 50 min.

[0046] The above-mentioned preparation method of lepidolite thermal insulation brick is further improved, in which in step S6, the product obtained after roasting is placed in water for leaching; the liquid-solid ratio is controlled to be 0.8-1:1 during the leaching process; and the leaching time is 3 to 4 days.

[0047] The above-mentioned method for preparing the lepidolite thermal insulation brick is further improved, in which in step (3), the pressure during the pressing process is controlled to be 5MPa to 15MPa; the pressing time is 5s to 20s; and the curing time is 28 days.

[0048] Compared with the prior art, the advantages of the present invention are:

[0049] (1) In view of the low porosity, high density, high thermal conductivity, low strength and other deficiencies of the existing lithium mica slag, as well as the low compressive strength of the bricks and the poor insulation effect caused by the defects, the present invention creatively proposes a lithium mica particle insulation brick, the lithium mica particles used are lithium mica leached slag prepared by granulating, roasting and leaching lithium mica as raw materials, the lithium mica leached slag is a porous particle with rich pore structure, with low density, high porosity, low thermal conductivity, high strength and other characteristics, so after compounding it with cement, the lithium mica particles can be closely combined by the bonding effect of cement, and further, by optimizing the amount of the two, a lithium mica particle insulation brick with light weight, high compressive strength and excellent insulation performance can be formed. In addition, a large amount of lithium mica particles are needed in the lithium mica particle insulation brick of the present invention, and by consuming a large amount of lithium mica particles, the land usage occupied by storage and the adverse effects on the ecological environment can also be reduced, which is conducive to reducing the risk of secondary pollution.

[0050] (2) The present invention also provides a method for preparing a lithium mica thermal insulation brick, wherein cement and water are first made into a slurry, and then lithium mica particles are added to form a mixture, and finally the mixture is pressed and formed, and cured to obtain a lithium mica thermal insulation brick with light weight, high compressive strength, and excellent thermal insulation performance. The preparation method of the present invention can use the lithium mica particles directly without the need for pretreatment such as grinding and drying the lithium mica particles. The preparation process is simpler, the operation is more convenient, the production energy consumption is lower, and it is suitable for large-scale preparation, which is convenient for realizing the industrial application of lithium mica thermal insulation bricks. Moreover, the amount of lithium mica particles used is large, which can realize the large-scale resource utilization of lithium mica particles, and can solve the waste of resources and environmental problems caused by the large-scale storage of lithium mica particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0052] Figure 1 The present invention is a schematic diagram of the preparation process of the lithium mica thermal insulation brick in Example 1. DETAILED DESCRIPTION

[0053] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby. The materials and instruments used in the following embodiments are all commercially available unless otherwise specified.

[0054] Example 1

[0055] A lithium mica thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0056] Lepidolite particles 40%,

[0057] Cement 60%.

[0058] In this embodiment, the lithium mica particles are leached slag produced by smelting lithium carbonate from lithium mica, and the main chemical components are: SiO2 content 35-45wt%, Fe2O3 content 7-10%, CaO content 10-14%; the mica particles contain 10-30% water, and the particle size distribution is between 5-10mm. Specifically, the lithium mica particles used are prepared by granulating, roasting and leaching lithium mica as raw material, comprising the following steps:

[0059] S1, take 100 kg of lithium mica concentrate (100 mesh, lithium mass percentage is 2%), according to the mass ratio of lithium ore concentrate to roasting additive is 1:0.6, wherein the roasting additive is a mixture of calcium sulfate, calcium carbonate, sodium sulfate and potassium sulfate, and the mass ratio of lithium mica concentrate to calcium sulfate, calcium carbonate, sodium sulfate, potassium sulfate is 1:0.3:0.1:0.1:0.1, so that the lithium mica concentrate and the roasting additive are evenly mixed and fully contacted to obtain mixed material A. In the present invention, the type of roasting additive and the dosage ratio of different types of roasting additives are adjusted according to actual conditions.

[0060] S2, according to the addition amount of roasting auxiliary material is 3% of the total mass of mixture A, mixture A is mixed with roasting auxiliary material (blue charcoal), and under the action of blue charcoal, lithium mica concentrate and roasting additive are bonded together to obtain mixture B, and blue charcoal in the mixture B. In the present invention, lithium ore concentrate is first mixed with the roasting additive, and then a volatile binder is added, which is not only more conducive to forming a material with good mixing uniformity, but also conducive to increasing the contact area between the lithium mica concentrate and the roasting additive.

[0061] S3. Add the mixed material B into a ball mill and grind the mixed material B until the particle size reaches 300 meshes to obtain a mixed material C.

[0062] S4. Mix the mixture C with water in an amount of 8% of the total mass of the mixture C to obtain a mixture D.

[0063] S5. The mixed material D is granulated by a disc granulator to obtain lithium mica concentrate particles with a particle size of 10 mm.

[0064] S6. Roasting the lithium ore concentrate particles in a rotary kiln, wherein the roasting temperature is 900° C. and the time is 45 minutes.

[0065] S7. The product obtained after calcination was placed in water for leaching at a liquid-to-solid ratio of 0.8:1 for 4 days, and solid-liquid separation was performed to obtain lithium mica particles.

[0066] In this embodiment, cement is composite silicate cement (commercially available).

[0067] A method for preparing the lithium mica thermal insulation brick in the above embodiment, the preparation process flow chart is as follows Figure 1 As shown, the following steps are included:

[0068] (1) Add cement into a mixer and stir. During the stirring process, add water accounting for 20% of the mass of the cement and mix well to obtain a slurry.

[0069] (2) Adding lepidolite particles to the slurry and stirring evenly to obtain a mixture of cement and lepidolite particles, wherein the mass ratio of lepidolite particles to cement in the mixture is 2:3.

[0070] (3) The mixture is injected into a molding machine, pressed at a pressure of 5 MPa for 15 seconds, and demolded to form thermal insulation bricks.

[0071] (4) The thermal insulation brick blanks are placed at room temperature for curing and solidified for 28 days to obtain finished lepidolite thermal insulation bricks.

[0072] Example 2

[0073] A lithium mica thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0074] Lepidolite particles 50%,

[0075] Cement 50%.

[0076] In this embodiment, the lithium mica particles used are the same as those in Example 1.

[0077] In this embodiment, the cement used is the same as that in Example 1.

[0078] A method for preparing the lepidolite thermal insulation brick in the present embodiment comprises the following steps:

[0079] (1) Add cement into a mixer and stir. During the stirring process, add water accounting for 20% of the mass of the cement and mix well to obtain a slurry.

[0080] (2) Adding lepidolite particles to the slurry and stirring evenly to obtain a mixture of cement and lepidolite particles, wherein the mass ratio of lepidolite particles to cement in the mixture is 1:1.

[0081] (3) The mixture is injected into a molding machine, pressed at a pressure of 5 MPa for 15 seconds, and demolded to form thermal insulation bricks.

[0082] (4) The thermal insulation brick blanks are placed at room temperature for curing and solidified for 28 days to obtain finished lepidolite thermal insulation bricks.

[0083] Example 3

[0084] A lithium mica thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0085] Lepidolite particles 60%,

[0086] Cement 40%.

[0087] In this embodiment, the lithium mica particles used are the same as those in Example 1.

[0088] In this embodiment, the cement used is the same as that in Example 1.

[0089] A method for preparing the lepidolite thermal insulation brick in the present embodiment comprises the following steps:

[0090] (1) Add cement into a mixer and stir. During the stirring process, add water accounting for 20% of the mass of the cement and mix well to obtain a slurry.

[0091] (2) Adding lepidolite particles to the slurry and stirring evenly to obtain a mixture of cement and lepidolite particles, wherein the mass ratio of lepidolite particles to cement in the mixture is 3:2.

[0092] (3) The mixture is injected into a molding machine, pressed at a pressure of 5 MPa for 15 seconds, and demolded to form thermal insulation bricks.

[0093] (4) The thermal insulation brick blanks are placed at room temperature for curing and solidified for 28 days to obtain finished lepidolite thermal insulation bricks.

[0094] Example 4

[0095] A lithium mica thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0096] Lepidolite particles 80%,

[0097] Cement 20%.

[0098] In this embodiment, the lithium mica particles used are the same as those in Example 1.

[0099] In this embodiment, the cement used is the same as that in Example 1.

[0100] A method for preparing the lepidolite thermal insulation brick in the present embodiment comprises the following steps:

[0101] (1) Add cement into a mixer and stir. During the stirring process, add water accounting for 20% of the mass of the cement and mix well to obtain a slurry.

[0102] (2) Adding lepidolite particles to the slurry and stirring evenly to obtain a mixture of cement and lepidolite particles, wherein the mass ratio of lepidolite particles to cement in the mixture is 4:1.

[0103] (3) The mixture is injected into a molding machine, pressed at a pressure of 5 MPa for 15 seconds, and demolded to form thermal insulation bricks.

[0104] (4) The thermal insulation brick blanks are placed at room temperature for curing and solidified for 28 days to obtain finished lepidolite thermal insulation bricks.

[0105] Example 5

[0106] A lithium mica thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0107] Lepidolite particles 60%,

[0108] Cement 40%.

[0109] In this embodiment, the lithium mica particles used are the same as those in Example 1.

[0110] In this embodiment, the cement used is the same as that in Example 1.

[0111] A method for preparing the lepidolite thermal insulation brick in the present embodiment comprises the following steps:

[0112] (1) Cement is added into a mixer and stirred. During the stirring process, water accounting for 15% of the mass of the cement is added and mixed evenly to obtain a slurry.

[0113] (2) Adding lepidolite particles to the slurry and stirring evenly to obtain a mixture of cement and lepidolite particles, wherein the mass ratio of lepidolite particles to cement in the mixture is 3:2.

[0114] (3) The mixture is injected into a molding machine, pressed at a pressure of 10 MPa for 15 seconds, and demolded to form thermal insulation bricks.

[0115] (4) The thermal insulation brick blanks are placed at room temperature for curing and solidified for 28 days to obtain finished lepidolite thermal insulation bricks.

[0116] Example 6

[0117] A lithium mica thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0118] Lepidolite particles 60%,

[0119] Cement 40%.

[0120] In this embodiment, the lithium mica particles used are the same as those in Example 1.

[0121] In this embodiment, the cement used is the same as that in Example 1.

[0122] A method for preparing the lepidolite thermal insulation brick in the present embodiment comprises the following steps:

[0123] (1) Cement is added into a mixer and stirred. During the stirring process, water accounting for 12% of the mass of the cement is added and mixed evenly to obtain a slurry.

[0124] (2) Adding lepidolite particles to the slurry and stirring evenly to obtain a mixture of cement and lepidolite particles, wherein the mass ratio of lepidolite particles to cement in the mixture is 3:2.

[0125] (3) The mixture is injected into a molding machine, pressed at a pressure of 15 MPa for 15 seconds, and demolded to form thermal insulation bricks.

[0126] (4) The thermal insulation brick blanks are placed at room temperature for curing and solidified for 28 days to obtain finished lepidolite thermal insulation bricks.

[0127] Example 7

[0128] A lithium mica thermal insulation brick is made of the following raw materials in terms of mass percentage:

[0129] Lepidolite particles 80%,

[0130] Cement 20%.

[0131] In this embodiment, the lithium mica particles used are the same as those in Example 1.

[0132] In this embodiment, the cement used is the same as that in Example 1.

[0133] A method for preparing the lepidolite thermal insulation brick in the present embodiment comprises the following steps:

[0134] (1) Cement is added into a mixer and stirred. During the stirring process, water accounting for 15% of the mass of the cement is added and mixed evenly to obtain a slurry.

[0135] (2) Adding lepidolite particles to the slurry and stirring evenly to obtain a mixture of cement and lepidolite particles, wherein the mass ratio of lepidolite particles to cement in the mixture is 4:1.

[0136] (3) The mixture is injected into a molding machine, pressed at a pressure of 15 MPa for 15 seconds, and demolded to form thermal insulation bricks.

[0137] (4) The thermal insulation brick blanks are placed at room temperature for curing and solidified for 28 days to obtain finished lepidolite thermal insulation bricks.

[0138] Comparative Example 1

[0139] A lepidolite slag insulation brick and a preparation method thereof are basically the same as those in Example 1, except that: in Comparative Example 1, lepidolite slag is used instead of lepidolite particles, wherein the lepidolite slag is leached slag obtained by leaching traditional powder materials, and specifically, lepidolite and sulfate are used as raw materials, and mixing, roasting, water leaching, and solid-liquid separation are carried out in sequence to obtain the lepidolite slag.

[0140] Comparative Example 2

[0141] A lepidolite slag insulation brick and a preparation method thereof are basically the same as those in Example 4, except that: in Comparative Example 2, lepidolite slag is used instead of lepidolite particles, wherein the lepidolite slag is leached slag obtained by leaching traditional powders, and specifically, lepidolite and sulfate are used as raw materials, and mixing, roasting, water leaching, and solid-liquid separation are carried out in sequence to obtain the lepidolite slag.

[0142] Test: According to GB / T 2542-2012 "Test Method for Wall Bricks", the compressive strength of the test specimens was tested under standard conditions for 7d and 28d of curing. The compressive strength, antifreeze strength and thermal conductivity test results of the lepidolite particle insulation bricks prepared in Examples 1-7 and the lepidolite slag insulation bricks prepared in Comparative Examples 1-2 are shown in Table 1.

[0143] Table 1 Compressive strength, thermal conductivity and density test values ​​of each insulation brick in Examples 1-7 and Comparative Examples 1-2

[0144]

[0145]

[0146] It can be seen from the data in Table 1 that compared with the conventional lithium mica slag insulation bricks obtained from powdered lithium mica slag, the lithium mica particle insulation bricks prepared from lithium mica particles in the present invention have higher compressive strength and better thermal insulation performance. This is because the lithium mica particles used in the present invention have the characteristics of low density, large porosity, low thermal conductivity, high strength, etc., and are porous particles with rich pore structure. When used to prepare insulation bricks, they can not only play a good insulation role in the insulation bricks, but also play a supporting role in the insulation bricks, significantly improving the strength of the bricks, especially the compressive strength. The compressive strength of the lithium mica particle insulation bricks is greater than 20MPa, and the thermal conductivity is less than 0.3W / (m·K). Obviously, this is not available in conventional lithium mica slag insulation bricks.

[0147] As can be seen from the above results, in the present invention, using lithium mica particles with low density, high porosity, low thermal conductivity and high strength as raw materials, it is a porous particle rich in pore structure, and only the bonding effect of cement is needed to closely combine lithium mica particles, and form lithium mica particles insulation bricks with light weight, high compressive strength and excellent thermal insulation performance. At the same time, the lithium mica particles used can be directly used, without the need to grind and dry lithium mica particles, the preparation process is simpler, the operation is more convenient, the production energy consumption is lower, it is suitable for large-scale preparation, it is easy to realize the industrial application of lithium mica particles insulation bricks, and the lithium mica particles used are large in amount, and the bulk resource utilization of lithium mica particles can be realized, and the waste of resources and environmental problems caused by the large-scale storage of lithium mica particles can be solved. In the present invention, insulation bricks are prepared using lithium mica particles, a new path is provided for the treatment of lithium mica particles, the utilization rate of lithium mica smelting slag is improved, and huge environmental benefits are brought.

[0148] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A lithium mica thermal insulation brick, characterized in that: The lithium mica thermal insulation brick is made of the following raw materials according to mass percentage: Lepidolite particles 40% to 80%, Cement 20%~60%; The lepidolite particles are prepared by using lepidolite as a raw material through granulation, roasting and leaching.

2. The lepidolite thermal insulation brick according to claim 1, characterized in that: The preparation method of the lithium mica particles comprises the following steps: S1, mixing lepidolite concentrate, a roasting additive and a volatile binder to obtain a mixture B; S2, finely grinding the mixture B until the particle size is above 200 meshes to obtain the mixture C; S3, mixing mixed material C with water to obtain mixed material D; S4, granulating the mixed material D to obtain lepidolite concentrate particles; S5, roasting the lithium ore concentrate particles; S6. Leaching the product obtained after roasting, separating the solid from the liquid, and obtaining lithium mica particles.

3. The lepidolite thermal insulation brick according to claim 2, characterized in that: In step S1, the mass ratio of the lithium mica concentrate to the roasting additive is 1:0.1-0.8; the amount of the volatile binder added is 1%-10% of the total mass of the lithium mica concentrate and the roasting additive; the roasting additive is at least one of calcium sulfate, calcium carbonate, sodium sulfate and potassium sulfate or a mixture thereof; the mass percentage of lithium in the lithium ore concentrate is ≥1.5%; the volatile binder is at least one of semi-coke and petroleum coke; In step S2, the particle size of the mixture C is 300 mesh to 1000 mesh; In step S3, the amount of water added is 5% to 20% of the total mass of the mixture C; In step S4, the particle size of the lepidolite concentrate particles is 8 mm to 10 mm; In step S5, a rotary kiln is used to roast the lithium ore concentrate particles; the roasting temperature is 850° C. to 900° C.; the roasting time is 30 min to 50 min; In step S6, the product obtained after roasting is placed in water for leaching; during the leaching process, the liquid-to-solid ratio is controlled to be 0.8 to 1:1; and the leaching time is 3 to 4 days.

4. The lepidolite thermal insulation brick according to any one of claims 1 to 3, characterized in that: The lithium mica thermal insulation brick is made of the following raw materials according to mass percentage: Lepidolite particles 60% to 80%, Cement 20%~40%.

5. The lepidolite thermal insulation brick according to claim 4, characterized in that: The particle size of the lithium mica particles is distributed between 5 mm and 10 mm; the cement is at least one of composite silicate cement, slag silicate cement, fly ash silicate cement and ferroaluminate cement.

6. A method for preparing a lithium mica thermal insulation brick, characterized in that: The following steps are involved: (1) Mixing cement and water and stirring to obtain slurry; (2) adding lithium mica particles to the slurry and stirring to obtain a mixture; the lithium mica particles are prepared by granulating, roasting and leaching lithium mica as a raw material; (3) The mixture is pressed into shape and cured to obtain lithium mica thermal insulation bricks.

7. The method for preparing the lepidolite thermal insulation brick according to claim 6, characterized in that: In step (1), the amount of water added is 12% to 20% of the mass of cement; the cement is at least one of composite silicate cement, slag silicate cement, fly ash silicate cement, and ferroaluminate cement; In step (2), the mass ratio of the lithium mica particles to the cement in the mixture is 2-4:1-3; and the particle size distribution of the lithium mica particles is between 5 mm and 10 mm.

8. The method for preparing the lepidolite thermal insulation brick according to claim 6 or 7, characterized in that: In step (2), the preparation method of the lithium mica particles comprises the following steps: S1, mixing lepidolite concentrate, a roasting additive and a volatile binder to obtain a mixture B; S2, finely grinding the mixture B until the particle size is above 200 meshes to obtain the mixture C; S3, mixing mixed material C with water to obtain mixed material D; S4, granulating the mixed material D to obtain lepidolite concentrate particles; S5, roasting the lithium ore concentrate particles; S6. Leaching the product obtained after roasting, separating the solid from the liquid, and obtaining lithium mica particles.

9. The method for preparing the lepidolite thermal insulation brick according to claim 8, characterized in that: In step S1, the mass ratio of the lithium mica concentrate to the roasting additive is 1:0.1-0.8; the amount of the volatile binder added is 1%-10% of the total mass of the lithium mica concentrate and the roasting additive; the roasting additive is at least one of calcium sulfate, calcium carbonate, sodium sulfate and potassium sulfate or a mixture thereof; the mass percentage of lithium in the lithium ore concentrate is ≥1.5%; the volatile binder is at least one of semi-coke and petroleum coke; In step S2, the particle size of the mixture C is 300 mesh to 1000 mesh; In step S3, the amount of water added is 5% to 20% of the total mass of the mixture C; In step S4, the particle size of the lepidolite concentrate particles is 8 mm to 10 mm; In step S5, a rotary kiln is used to roast the lithium ore concentrate particles; the roasting temperature is 850° C. to 900° C.; the roasting time is 30 min to 50 min; In step S6, the product obtained after roasting is placed in water for leaching; during the leaching process, the liquid-to-solid ratio is controlled to be 0.8 to 1:1; and the leaching time is 3 to 4 days.

10. The method for preparing the lepidolite thermal insulation brick according to claim 6 or 7, characterized in that: In step (3), the pressure during the pressing process is controlled to be 5MPa to 15MPa; the pressing time is 5s to 20s; and the curing time is 28 days.

Citation Information

Patent Citations

  • Method for preparing light building material ceramsites by using lithium extraction slag of lithium mica

    CN102126838A

  • Ceramsite self-thermal-insulating building block and preparation method thereof

    CN103951342A

  • Lepidolite compression molding and roasting as well as lithium extracting method and device

    CN110983035A

  • Ceramsite acoustic board for metal sound barrier and preparation method and application of ceramsite acoustic board

    CN112608111A

  • Method for synergistically preparing baking-free steaming-free cured bricks from squeezed fine silt and lithium slag obtained after lepidolite beneficiation based on carbon curing

    CN114031341A