Concrete for highway and preparation method thereof

By using the crown ether-based polymer water reducing agent provided by reversible addition-break chain transfer polymerization in concrete, the problem of insufficient slump retention in high temperature environment is solved, the durability and compressive strength of concrete are improved, and the Stable performance at high temperatures.

CN118908644APending Publication Date: 2024-11-08HUBEI ZHONGKE HIGHWAY SURVEY & DESIGN INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410815651.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing polyether type or polycarboxylic acid type water reducing agents have insufficient slump retention and are sensitive to temperature in high temperature environments, making it difficult to maintain good performance in mixed soil.

Method used

Reversible addition-break chain transfer polymerization is used to provide a polymer with crown ether group as a water reducer. Through its chelation with metal ions and steric hindering, the dispersion of cement particles and concrete fluidity are improved and the porosity is reduced.

Benefits of technology

It significantly improves the durability and compressive strength of concrete, ensures good slump and expansion at high temperatures, and extends the service life of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004907522250000091
    Figure BDA0004907522250000091
  • Figure BDA0004907522250000111
    Figure BDA0004907522250000111
Patent Text Reader

Abstract

The invention relates to the technical field of concrete, in particular to highway concrete and a preparation method thereof. The concrete is prepared from the following raw materials in parts by weight: 200 to 450 parts of coarse aggregate, 150 to 300 parts of fine aggregate, 100 to 200 parts of cement, 10 to 30 parts of fiber material, 10 to 20 parts of binder, 5 to 15 parts of modified polycarboxylate superplasticizer and 150 to 250 parts of water. The invention also provides a preparation method of the composition. Compared with the prior art, the concrete prepared by the invention has the advantages of better slump retaining property at high temperature, excellent durability and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete, and in particular to a highway concrete and a preparation method thereof. Background Art

[0002] Concrete's plasticity, high durability, designability of strength, and low cost make it the most widely used building material. However, concrete is prone to cracking due to self-drying and differences in ambient temperature and humidity. This phenomenon is particularly evident in the interface transition zone, where cracks may have already occurred before loading. The occurrence of cracks is related to the amount and type of cementitious materials, water-cement ratio, type and gradation of aggregates, curing conditions, and admixtures. Improper design will increase the number and size of cracks, thereby reducing the durability of concrete. Water reducers play an important role in improving the durability of concrete. It reduces the water-cement ratio, reduces the amount of cement slurry, and increases the density of concrete, thereby enhancing the concrete's impermeability, freeze-thaw resistance, and chemical erosion resistance. The use of water reducers can also reduce the shrinkage and cracks of concrete, improve the protection of steel bars, and extend the service life of concrete structures. In addition, it improves the workability of concrete, ensures that concrete is easier to pour and compact during construction, reduces construction defects, and improves the overall durability of concrete structures. Therefore, water reducers are important additives for improving the long-term performance and service life of concrete.

[0003] CN202011228538.X discloses a concrete and a preparation method thereof, comprising the following components by mass: 14-20% of silicate cement, 6-10% of active fly ash, 3-5% of copper tailings powder, 0.2-0.4% of magnesium hydroxide, 0.4-0.8% of sodium chloride, 0.8-1.7% of modified basalt fiber, 25-30% of crushed stone, 28.3-37.9% of waste tile sand, 0.5-1% of modified polycarboxylate ether water reducer, and 8-10.5% of water. The preparation method of the invention is reliable and easy to implement, and the obtained concrete has low cost, good early strength, workability, pumpability and crack resistance.

[0004] CN202111236335.X belongs to the field of concrete technology, and specifically relates to a durable concrete, including the following components in parts by weight: 300-400 parts of cement, 450-550 parts of fine aggregate, 720-820 parts of coarse aggregate, 100-200 parts of water, 20-40 parts of fiber, 20-40 parts of polymer emulsion, and 10-20 parts of polycarboxylate water reducer. The durable concrete of this application can enhance the impact toughness of concrete materials by adding flexible fibers to the base material, and play an effective role in preventing cracks and seepage. In addition, the added polycarboxylate water reducer has a phenyl o-hydroxybenzoate structure that can absorb ultraviolet rays. The ultraviolet absorption structure is bonded to the polycarboxylate water reducer and is not easy to migrate or precipitate like small molecule ultraviolet absorbers, thereby playing a long-term anti-aging role and improving the durability of concrete.

[0005] Water reducers can significantly improve the density of concrete and reduce permeability, playing an important role in extending its service life. However, current polyether or polycarboxylic acid water reducers still have problems such as insufficient slump retention and temperature sensitivity in high temperature environments, which need to be solved urgently. Summary of the invention

[0006] In view of the above-mentioned defects in the prior art, the technical problem to be solved by the present invention is to provide a highway concrete and a preparation method thereof.

[0007] Polycarboxylate water reducer (PCE) is a water reducer with good performance. Through the design of efficient molecular structure, the mechanism of action of dispersing cement is successfully realized. It shows low dosage, good water reduction, high fluidity, wide application range, high molecular structure, high degree of freedom, multi-channel synthesis process, excellent performance, huge development potential, so that concrete can be significantly strengthened and the shrinkage problem of concrete can be effectively reduced. The present invention provides a polymer with crown ether group as a water reducer through reversible addition-fragmentation chain transfer polymerization. The crown ether group has a large steric hindrance due to its special structure, and the ability to form a complex with metal ions, and the pores between cements are rich in metal ions such as sodium, potassium, and calcium. Therefore, the crown ether can be well chelated with these metal ions to achieve a steric stabilization effect, and its large steric hindrance prevents cement particles from approaching each other. The steric hindrance plays a leading role in the deflocculation of cement paste. The more obvious the steric hindrance is, the more conducive it is to the dispersion of cement particles. Therefore, the fluidity of cement paste is improved, so that the porosity of the obtained concrete is reduced and the durability is better.

[0008] In the present invention, coarse aggregate and fine aggregate together constitute the skeleton of concrete, providing structural support and strength. Cement, as a cementitious material, bonds aggregates into a solid whole through hydration reaction. The addition of fiber materials can play a role in reinforcement and toughening. The binder enhances the bonding force between aggregates and cement slurry, and improves the cohesion and durability of concrete. The addition of modified polycarboxylic acid water-reducing agent not only optimizes the workability of concrete, but also helps to improve its strength and durability. The right amount of water ensures the full hydration of cement and is the key to forming a concrete structure.

[0009] To achieve the above object, the present invention provides a highway concrete, comprising the following raw materials in parts by weight: 200-450 parts of coarse aggregate, 150-300 parts of fine aggregate, 100-200 parts of cement, 10-30 parts of fiber material, 10-20 parts of binder, 5-15 parts of modified polycarboxylic acid water reducer and 150-250 parts of water.

[0010] Furthermore, the coarse aggregate is crushed stone with a particle size of 5mm to 30mm.

[0011] Furthermore, the fine aggregate is river sand with a particle size of 0.5 to 0.35 mm.

[0012] Furthermore, the cement is one of silicate cement, ordinary silicate cement, slag silicate cement and pozzolanic silicate cement.

[0013] Furthermore, the fiber material is one of steel fiber, glass fiber, nylon fiber, polypropylene fiber and polyethylene fiber.

[0014] Furthermore, the binder is polyvinyl acetate or polyurethane latex.

[0015] The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:

[0016] X1. Add 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene to dioxane, heat to 70-80° C. under an inert atmosphere, stir for 16-28 hours, then cool and quench, add acetone to dilute the reaction solution, and precipitate with ether, filter and dry for the next step;

[0017] X2. Add the product of the previous step to N,N-dimethylformamide, then add dibenzo-15-crown-5,4-dimethylaminopyridine, heat to 70-80°C and stir for 16-32h. After cooling to room temperature, add dilute hydrochloric acid to dilute the precipitate, filter it, wash the residue with acid, dissolve it in acetone, dilute it with ether, filter it, and dry it.

[0018] Furthermore, the molar ratio of the 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid, and trioxymethylene is 1:1-1.2:0.001-0.005:2-2.5:0.1-0.2.

[0019] Furthermore, in step X2, the molar ratio of the product of the previous step to dibenzo-15-crown-5,4-dimethylaminopyridine is 1:1-2:0.1-0.3.

[0020] Preferably, the preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:

[0021] X1. Add 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene in a molar ratio of 1:1-1.2:0.001-0.005:2-2.5:0.1-0.2 to dioxane, heat to 70-80°C under an inert atmosphere, stir for 16-28h, then cool and quench, add acetone to dilute the reaction solution, and precipitate with ether, filter and dry for the next step;

[0022] X2. Add the product of the previous step to N,N-dimethylformamide, and then add dibenzo-15-crown-5,4-dimethylaminopyridine. The molar ratio of the product of the previous step to dibenzo-15-crown-5,4-dimethylaminopyridine is 1:1~2:0.1~0.3. Heat to 70~80℃ and stir for 16~32h. After cooling to room temperature, add dilute hydrochloric acid to dilute and precipitate. Filter. Wash the residue with acid, dissolve it in acetone, dilute it with ether, filter it, and dry it.

[0023] A method for preparing highway concrete comprises the following steps:

[0024] S1. Mix cement, fine aggregate, coarse aggregate and fiber material in proportion, stir evenly to obtain a mixture;

[0025] S2, adding the modified polycarboxylic acid water-reducing agent and the binder into the mixing water, stirring evenly to obtain a mixed solution;

[0026] S3, mixing the mixed liquid with the mixed material and stirring evenly to obtain.

[0027] Beneficial effects of the present invention:

[0028] 1. Compared with the prior art, the present invention provides a polymer having a crown ether group as a water reducer through reversible addition-fragmentation chain transfer polymerization. The crown ether can chelate with these metal ions well, thereby achieving a spatial stabilization effect, and its large steric hindrance prevents cement particles from approaching each other. The steric hindrance plays a leading role in the deflocculation of cement paste. The more obvious the steric hindrance is, the more conducive it is to the dispersion of cement particles. Therefore, the fluidity of the cement paste is improved, so that the porosity of the obtained concrete is reduced and the durability is better.

[0029] 2. The present invention uses coarse aggregate and fine aggregate to form the skeleton of concrete, providing structural support and strength. Cement, as a cementitious material, bonds aggregates into a solid whole through hydration reaction. The addition of fiber materials can play a role in reinforcement and toughening. The binder enhances the bonding force between aggregates and cement slurry, and improves the cohesion and durability of concrete. The addition of modified polycarboxylic acid water-reducing agent not only optimizes the workability of concrete, but also helps to improve its strength and durability. The right amount of water ensures the full hydration of cement and is the key to forming a concrete structure. . DETAILED DESCRIPTION

[0030] Ordinary Portland cement, P.O42.5, Shaoxing Yaowei Building Materials.

[0031] Polyethylene fiber, 12mm, Guangzhou Zhangdao Chemical.

[0032] Polyvinyl acetate, item number: HS1801, Foshan Nanhai Jiangshun Chemical Products.

[0033] The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:

[0034] X1. Add 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene to dioxane, heat to 70-80° C. under an inert atmosphere, stir for 16-28 hours, then cool and quench, add acetone to dilute the reaction solution, and precipitate with ether, filter and dry for the next step;

[0035] X2. Add the product of the previous step to N,N-dimethylformamide, then add dibenzo-15-crown-5,4-dimethylaminopyridine, heat to 70-80°C and stir for 16-32h. After cooling to room temperature, add dilute hydrochloric acid to dilute the precipitate, filter it, wash the residue with acid, dissolve it in acetone, dilute it with ether, filter it, and dry it.

[0036] 2-Ethyl acrylic acid and pentafluorophenol acrylate are polymerized with azobisisobutyronitrile as the initiator in the presence of dioxane as the medium, and 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid is used as a chain transfer agent to obtain a copolymer with active esters, and then ester exchange is carried out with dibenzo-15-crown-5 and 4-dimethylaminopyridine to obtain the modified polycarboxylic acid water reducer.

[0037] Comparative Example 1

[0038] A method for preparing highway concrete comprises the following steps:

[0039] S1, mix 1.5kg of ordinary Portland cement, 2kg of river sand, 4kg of crushed stone and 0.2kg of polyethylene fiber, stir evenly to obtain a mixture;

[0040] S2, adding 0.15 kg of polyvinyl acetate to 2 kg of mixing water, stirring evenly to obtain a mixed solution;

[0041] S3, mixing the mixed liquid with the mixed material and stirring evenly to obtain.

[0042] Example 1

[0043] A method for preparing highway concrete comprises the following steps:

[0044] S1, mix 1.5kg of ordinary Portland cement, 2kg of river sand, 4kg of crushed stone and 0.2kg of polyethylene fiber, stir evenly to obtain a mixture;

[0045] S2. Add 0.1 kg of modified polycarboxylate water reducer and 0.15 kg of polyvinyl acetate into 2 kg of mixing water, stir evenly to obtain a mixed solution;

[0046] S3, mixing the mixed liquid with the mixed material and stirring evenly to obtain.

[0047] The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:

[0048] X1. Add 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene in a molar ratio of 1:1:0.003:2:0.15 to dioxane, heat to 70°C under an inert atmosphere and stir for 20 hours, then cool and quench, add acetone to dilute the reaction solution, and use ether to precipitate, filter and dry for the next step;

[0049] X2. Add the product of the previous step to N,N-dimethylformamide, and then add dibenzo-15-crown-5,4-dimethylaminopyridine. The molar ratio of the product of the previous step to dibenzo-15-crown-5,4-dimethylaminopyridine is 1:1.5:0.2. Heat to 80°C and stir for 24 hours. After cooling to room temperature, add dilute hydrochloric acid to dilute and precipitate. Filter. Wash the residue with acid, dissolve it in acetone, dilute it with ether, filter it, and dry it.

[0050] Example 2

[0051] A method for preparing highway concrete comprises the following steps:

[0052] S1, mix 1.5kg of ordinary Portland cement, 2kg of river sand, 4kg of crushed stone and 0.2kg of polyethylene fiber, stir evenly to obtain a mixture;

[0053] S2. Add 0.1 kg of modified polycarboxylate water reducer and 0.15 kg of polyvinyl acetate into 2 kg of mixing water, stir evenly to obtain a mixed solution;

[0054] S3, mixing the mixed liquid with the mixed material and stirring evenly to obtain.

[0055] The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:

[0056] 2-Ethyl acrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene are added to dioxane in a molar ratio of 1:1:0.003:2:0.15, heated to 70°C under an inert atmosphere and stirred for 20 hours, then cooled and quenched, acetone is added to dilute the reaction solution, and ether is used to precipitate, which is filtered and dried to obtain the product.

[0057] Example 3

[0058] A method for preparing highway concrete comprises the following steps:

[0059] S1, mix 1.5kg of ordinary Portland cement, 2kg of river sand, 4kg of crushed stone and 0.2kg of polyethylene fiber, stir evenly to obtain a mixture;

[0060] S2. Add 0.1 kg of modified polycarboxylate water reducer and 0.15 kg of polyvinyl acetate into 2 kg of mixing water, stir evenly to obtain a mixed solution;

[0061] S3, mixing the mixed liquid with the mixed material and stirring evenly to obtain.

[0062] The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:

[0063] X1. Add 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene in a molar ratio of 1:1:0.003:2:0.15 to dioxane, heat to 70°C under an inert atmosphere and stir for 20 hours, then cool and quench, add acetone to dilute the reaction solution, and use ether to precipitate, filter and dry for the next step;

[0064] X2. Add the product of the previous step to N,N-dimethylformamide, and then add 12-crown-4,4-dimethylaminopyridine. The molar ratio of the product of the previous step to 12-crown-4,4-dimethylaminopyridine is 1:1.5:0.2. Heat to 80°C and stir for 24 hours. After cooling to room temperature, add dilute hydrochloric acid to dilute and precipitate. Filter. Wash the residue with acid, dissolve it in acetone, dilute it with ether, filter it, and dry it.

[0065] Example 4

[0066] A method for preparing highway concrete comprises the following steps:

[0067] S1, mix 1.5kg of ordinary Portland cement, 2kg of river sand, 4kg of crushed stone and 0.2kg of polyethylene fiber, stir evenly to obtain a mixture;

[0068] S2. Add 0.1 kg of modified polycarboxylate water reducer and 0.15 kg of polyvinyl acetate into 2 kg of mixing water, stir evenly to obtain a mixed solution;

[0069] S3, mixing the mixed liquid with the mixed material and stirring evenly to obtain.

[0070] The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:

[0071] X1. Add 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene in a molar ratio of 1:1:0.003:2:0.15 to dioxane, heat to 70°C under an inert atmosphere and stir for 20 hours, then cool and quench, add acetone to dilute the reaction solution, and use ether to precipitate, filter and dry for the next step;

[0072] X2. Add the product of the previous step to N,N-dimethylformamide, and then add 15-crown-5,4-dimethylaminopyridine. The molar ratio of the product of the previous step to 15-crown-5,4-dimethylaminopyridine is 1:1.5:0.2. Heat to 80°C and stir for 24 hours. After cooling to room temperature, add dilute hydrochloric acid to dilute and precipitate. Filter. Wash the residue with acid, dissolve it in acetone, dilute it with ether, filter it, and dry it.

[0073] Example 5

[0074] A method for preparing highway concrete comprises the following steps:

[0075] S1, mix 1.5kg of ordinary Portland cement, 2kg of river sand, 4kg of crushed stone and 0.2kg of polyethylene fiber, stir evenly to obtain a mixture;

[0076] S2, adding 0.1 kg of modified polycarboxylate water reducer and 0.15 kg of polyvinyl acetate into 2 kg of mixing water, stirring evenly to obtain a mixed solution;

[0077] S3, mixing the mixed liquid with the mixed material and stirring evenly to obtain.

[0078] The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:

[0079] X1. Add 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene in a molar ratio of 1:1:0.003:2:0.15 to dioxane, heat to 70°C under an inert atmosphere and stir for 20 hours, then cool and quench, add acetone to dilute the reaction solution, and use ether to precipitate, filter and dry for the next step;

[0080] X2. Add the product of the previous step to N,N-dimethylformamide, and then add 18-crown-6,4-dimethylaminopyridine, the molar ratio of the product of the previous step to 18-crown-6,4-dimethylaminopyridine is 1:1.5:0.2, heat to 80°C and stir for 24 hours, cool to room temperature, add dilute hydrochloric acid to dilute, and precipitate. Filter, wash the residue with acid, dissolve in acetone, dilute with ether, filter, and dry.

[0081] Test Example 1

[0082] According to the relevant provisions of GB 8076-2008 "Concrete Admixtures", the slump / expansion, air content and compressive strength of concrete are tested. The concrete slump / expansion test is to mix the concrete at a high temperature of 35°C to obtain a sample and then divide it into three layers evenly and place it in a slump cone. The height of each layer is about one-third of the cone height. The slump cone is lifted vertically, and the difference between the height of the slump cone and the height of the highest point on the concrete surface is measured to obtain the slump value of the concrete. The concrete mixture is placed in a measuring bowl, and water is injected. Wait until the water from the outlet of the exhaust valve reaches a uniform speed, and then close the water inlet valve and the exhaust valve. Pressurize the inside, press the pressure valve two or three times, and the value obtained by reading the meter is the air content. Prepare samples by moduleizing the concrete, then cure, take out the samples and demould, and use a compressive strength testing machine to measure the compressive strength of the samples.

[0083] Table 1 Concrete performance test results

[0084]

[0085] In practical applications, when testing the viscosity of concrete, the expansion of concrete can be used as a criterion. It can be seen from the performance test that the concrete prepared by the embodiment still has a better slump / expansion under high temperature mixing than the control example, indicating that the prepared concrete has good workability. This may be because the water reducer used in the embodiment can be adsorbed on the surface of cement, so that the cement particles are separated from each other, so that the free water wrapped inside the cement particles can be released, achieving the purpose of water reduction, and improving the fluidity of gel materials such as cement. Compared with Examples 3 to 5, Example 1 shows that the performance deteriorates with the increase of the crown ether structure. Example 1 is relatively the best. This may be because the steric hindrance effect also plays a key role in concrete. When the water reducer is adsorbed on the surface of cement particles, the side chain of the water reducer extends into the liquid phase to form an adsorption layer, generating a steric hindrance effect, and preventing cement particles from approaching each other. The more the adsorption layers overlap, the greater the steric repulsion. Therefore, the magnitude of this force is closely related to the side chain of the water reducer. When the side chain length increases, the adsorption layer on the cement particles becomes thicker, the steric hindrance becomes more obvious, and the more conducive to the dispersion of cement particles, the fluidity of cement paste is improved. However, it can be seen from the test data that the magnitude of this force does not increase infinitely. When the crown ether size is too large, the performance decreases instead. This may be because the steric hindrance is too large and affects the adsorption of cement particles. However, compared with Example 4, the structure of the crown ether in Example 1 remains unchanged, with only 2 more benzene rings, so the steric hindrance is not significantly increased compared with Example 5, but the increase in benzene rings can further improve thermal stability. This is very important for the water reducer to maintain good slump retention under high temperature mixing. Therefore, the performance of Example 1 is better than that of Example 4. Due to its special structure, the crown ether group has a large steric hindrance, good thermal stability at high temperature and the ability to form complexes with metal ions. The pores between cement are rich in metal ions such as sodium, potassium, and calcium. Therefore, the crown ether can chelate with these metal ions well, thereby achieving a steric stabilization effect. Its large steric hindrance prevents cement particles from approaching each other. Steric hindrance plays a leading role in the deflocculation of cement paste. The more obvious the steric hindrance is, the more conducive it is to the dispersion of cement particles. Therefore, the fluidity of the cement paste is improved, thereby reducing the porosity of the resulting concrete and thus having high compressive strength.

[0086] Test Example 2

[0087] The control example and the embodiment were subjected to durability tests, and the compressive strength loss rate after freeze-thaw cycles was determined according to GB / T50082-2009 "Test methods for long-term performance and durability of ordinary concrete".

[0088] Table 2 Concrete permeability coefficient and durability test

[0089]

[0090] It can be seen from the test results that the concrete prepared by the present invention has good durability. This may be because some embodiments provide a polymer with a crown ether group as a water reducer through reversible addition-fragmentation chain transfer polymerization. The crown ether group has a large steric hindrance due to its special structure, and the ability to form a complex with metal ions. The pores between cements are rich in metal ions such as sodium, potassium, and calcium. Therefore, the crown ether can chelate with these metal ions well, thereby achieving a spatial stabilization effect, and its large steric hindrance prevents cement particles from approaching each other. The steric hindrance plays a leading role in the deflocculation of cement paste. The more obvious the steric hindrance is, the more conducive it is to the dispersion of cement particles. Therefore, the fluidity of the cement paste is improved, so that the porosity of the obtained concrete is reduced and the durability is better.

[0091] In the present invention, coarse aggregate and fine aggregate together constitute the skeleton of concrete, providing structural support and strength. Cement, as a cementitious material, bonds aggregates into a solid whole through hydration reaction. The addition of fiber materials can play a role in reinforcement and toughening. The binder enhances the bonding force between aggregates and cement slurry, and improves the cohesion and durability of concrete. The addition of modified polycarboxylic acid water-reducing agent not only optimizes the workability of concrete, but also helps to improve its strength and durability. The right amount of water ensures the full hydration of cement and is the key to forming a concrete structure.

[0092] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A kind of concrete for highway, It is characterized in that The invention comprises the following raw materials in parts by weight: 200-450 parts of coarse aggregate, 150-300 parts of fine aggregate, 100-200 parts of cement, 10-30 parts of fiber material, 10-20 parts of binder, 5-15 parts of modified polycarboxylic acid water-reducing agent and 150-250 parts of water.

2. The highway concrete according to claim 1, It is characterized in that The coarse aggregate is crushed stone with a particle size of 5mm to 30mm.

3. The highway concrete according to claim 1, It is characterized in that The fine aggregate is river sand with a particle size of 0.5 to 0.35 mm.

4. The highway concrete according to claim 1, It is characterized in that The cement is one of silicate cement, ordinary silicate cement, slag silicate cement and pozzolanic silicate cement.

5. The road concrete according to claim 1, It is characterized in that The fiber material is one of steel fiber, glass fiber, nylon fiber, polypropylene fiber and polyethylene fiber.

6. The highway concrete according to claim 1, It is characterized in that The adhesive is polyvinyl acetate or polyurethane latex.

7. The road concrete according to claim 1, It is characterized in that The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps: X1. Add 2-ethylacrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene to dioxane, heat to 70-80° C. under an inert atmosphere, stir for 16-28 hours, then cool and quench, add acetone to dilute the reaction solution, and precipitate with ether, filter and dry for the next step; X2. Add the product of the previous step to N,N-dimethylformamide, then add dibenzo-15-crown-5,4-dimethylaminopyridine, heat to 70-80°C and stir for 16-32h. After cooling to room temperature, add dilute hydrochloric acid to dilute the precipitate, filter it, wash the residue with acid, dissolve it in acetone, dilute it with ether, filter it, and dry it.

8. The road concrete according to claim 7, It is characterized in that The molar ratio of the 2-ethyl acrylic acid, pentafluorophenol acrylate, azobisisobutyronitrile, 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and trioxymethylene is 1:1-1.2:0.001-0.005:2-2.5:0.1-0.

2.

9. The road concrete according to claim 7, It is characterized in that In the step X2, the molar ratio of the product of the previous step to dibenzo-15-crown-5,4-dimethylaminopyridine is 1:1-2:0.1-0.

3.

10. A method for preparing highway concrete according to any one of claims 1 to 9, It is characterized in that The steps include: S1. Mix cement, fine aggregate, coarse aggregate and fiber material in proportion, stir evenly to obtain a mixture; S2, adding the modified polycarboxylic acid water-reducing agent and the binder into the mixing water, stirring evenly to obtain a mixed solution; S3, mixing the mixed liquid with the mixed material and stirring evenly to obtain.