UHPC concrete and preparation method thereof
By combining modified garnet powder with polyacrylonitrile and o-hydroxybenzamide, the compressive strength and flexural strength of UHPC concrete are improved, and the problem of insufficient performance of existing UHPC concrete is solved, and the market demand for high performance is met .
Patent Information
- Application Number
- CN202411250619.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
AI Technical Summary
At present, UHPC concrete cannot meet the high requirements of the market for compressive strength and flexural strength.
Modified garnet powder is used to modify the garnet powder by polyacrylonitrile and o-hydroxybenzamide, and combined with cement, fume, basalt fiber, quartz sand and other components to improve the compressive strength and flexural strength of UHPC concrete.
It significantly improves the compressive strength and flexural strength of UHPC concrete, meeting the market's demand for high performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete, and in particular to UHPC concrete and a preparation method thereof. Background Art
[0002] UHPC concrete is an advanced building material with excellent durability and good working performance, so it is widely used in many fields. For example, in the field of civil engineering, such as bridges, tunnels, highway and railway bridges, UHPC can be used to make prestressed components with ultra-long life, improve the bearing capacity and seismic performance of the structure; in the field of high-rise buildings; UHPC can be used to make light and thin-walled structures to reduce the dead weight of the structure and seismic loads; in the field of architectural decoration, the delicate texture and plasticity of UHPC make it have broad application prospects in architectural decoration and landscape design.
[0003] Although UHPC concrete has many significant advantages, it also has some shortcomings in practical applications. With the increasing research and application of UHPC concrete, the market has put forward higher requirements for the compressive strength and flexural strength of UHPC concrete. The current UHPC concrete can no longer meet people's needs. Therefore, improving the compressive strength and flexural strength of UHPC concrete is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present invention provides a UHPC concrete and a preparation method thereof, which solves the problem of poor compressive strength and poor flexural strength of UHPC concrete in the related art.
[0005] The technical solution of the present invention is as follows: The present invention provides a UHPC concrete comprising the following components in parts by weight: 30-40 parts of cement, 8-10 parts of silica fume, 10-15 parts of basalt fiber, 35-65 parts of quartz sand, 28-40 parts of modified garnet powder, 1-3 parts of water reducer, 6-10 parts of water; The raw materials of the modified garnet powder include garnet powder and polyacrylonitrile.
[0006] As a further technical solution, the weight ratio of the garnet powder to the polyacrylonitrile is 8-17:1.
[0007] When the weight ratio of garnet powder to polyacrylonitrile is 8~17:1, it helps to further improve the compressive strength and flexural strength of UHPC concrete.
[0008] As a further technical solution, the preparation method of the modified garnet powder includes the following steps: dissolving the polyacrylonitrile in dimethylformamide to obtain a polyacrylonitrile solution, adding the garnet powder to the polyacrylonitrile solution, dispersing evenly, concentrating, and drying to obtain the modified garnet powder.
[0009] As a further technical solution, the polyacrylonitrile is divided into a first polyacrylonitrile and a second polyacrylonitrile, the molecular weight of the first polyacrylonitrile is 50,000, and the molecular weight of the second polyacrylonitrile is 150,000. The polyacrylonitrile adopts the first polyacrylonitrile and the second polyacrylonitrile with different molecular weights, and the first polyacrylonitrile and the second polyacrylonitrile are used together to further improve the compressive strength and flexural strength of UHPC concrete.
[0010] As a further technical solution, the weight ratio of the first polyacrylonitrile to the second polyacrylonitrile is 1-3:1.
[0011] When the weight ratio of the first polyacrylonitrile to the second polyacrylonitrile is 1-3:1, the compressive strength and flexural strength of the UHPC concrete can be further improved.
[0012] As a further technical solution, the mass fraction of the polyacrylonitrile solution is 6% to 12%.
[0013] As a further technical solution, the raw material of the modified garnet powder also includes o-hydroxybenzamide.
[0014] In the present invention, although the compressive strength and flexural strength of UHPC concrete can be improved by modifying garnet powder by polyacrylonitrile, the inventors found that when the raw material of the modified garnet powder also includes o-hydroxybenzamide, the compressive strength and flexural strength of UHPC concrete can be further improved by modifying the garnet powder by polyacrylonitrile and o-hydroxybenzamide.
[0015] As a further technical solution, the weight ratio of the garnet powder, polyacrylonitrile and o-hydroxybenzamide is 7-16:1:1.
[0016] When the weight ratio of garnet powder, polyacrylonitrile and o-hydroxybenzamide is 7~16:1:1, it helps to further improve the compressive strength and flexural strength of UHPC concrete.
[0017] As a further technical solution, the preparation method of the modified garnet powder comprises the following steps: A1, dissolving the polyacrylonitrile in dimethylformamide to obtain a polyacrylonitrile solution, adding the garnet powder to the polyacrylonitrile solution, dispersing the mixture evenly, concentrating the mixture, and drying the mixture to obtain a mixture; A2, dissolving the o-hydroxybenzamide in ethanol to obtain an o-hydroxybenzamide solution, adding the mixture to the o-hydroxybenzamide solution, dispersing evenly, concentrating, and drying to obtain modified garnet powder.
[0018] As a further technical solution, in step A1, the mass fraction of the polyacrylonitrile solution is 6% to 12%; in step A2, the mass fraction of the o-hydroxybenzamide solution is 8% to 10%.
[0019] As a further technical solution, the water reducer is one or both of sodium lignin sulfonate and polycarboxylic acid water reducer.
[0020] As a further technical solution, the particle size of the silica ash is 5-15 μm; the length of the basalt fiber is 4-8 mm and the diameter is 6-8 μm; the particle size of the quartz sand is 125-180 μm; and the particle size of the garnet powder is 35-45 μm.
[0021] The present invention also provides a method for preparing UHPC concrete, comprising the following steps: blending the remaining components except water and the water reducing agent, adding water and the water reducing agent, and mixing evenly to obtain UHPC concrete.
[0022] As a further technical solution, during the blending, the stirring speed is 150-200 r / min, and the stirring time is 10-15 min; when the mixing is uniform, the stirring speed is 1000-1500 r / min, and the stirring time is 5-10 min.
[0023] The working principle and beneficial effects of the present invention are: In the present invention, the raw materials of UHPC concrete include modified garnet powder. The garnet powder is modified by using polyacrylonitrile, which can improve the interface bonding between the garnet powder and the cement system, reduce the voids in the interface, and thus improve the compressive strength and flexural strength of the UHPC concrete. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] In the following embodiments and comparative examples, cement is ordinary Portland cement, model PW32.5; the particle size of silica fume is 10 μm; the length of basalt fiber is 6 mm and the diameter is 8 μm; the particle size of quartz sand is 125 μm; the particle size of garnet powder is 35 μm; the water reducer is sodium lignin sulfonate, and the effective content is 99 wt %; the model of the first polyacrylonitrile is PM05N, the model of the second polyacrylonitrile is PM15N, and the manufacturer is Hubei Chushengwei Chemical Co., Ltd.; the model of styrene-acrylonitrile copolymer is 90HR.
[0026] Example 1 A UHPC concrete comprises the following components in parts by weight: 30 parts of cement, 8 parts of silica fume, 10 parts of basalt fiber, 35 parts of quartz sand, 28 parts of modified garnet powder, 1 part of sodium lignin sulfonate, 6 parts of water; The raw materials of the modified garnet powder include 24 parts of garnet powder and 4 parts of polyacrylonitrile with a weight average molecular weight of 50,000; The preparation method of modified garnet powder comprises the following steps: dissolving 4 parts of polyacrylonitrile with a weight average molecular weight of 50,000 in dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 8%, adding 24 parts of garnet powder to the polyacrylonitrile solution with a mass fraction of 8%, dispersing evenly, concentrating, and drying to obtain modified garnet powder; The preparation method of UHPC concrete comprises the following steps: stirring the remaining components except water and the water reducing agent at a stirring speed of 150 r / min for 15 minutes, blending, adding water and the water reducing agent, stirring at a stirring speed of 1000 r / min for 10 minutes, mixing evenly, and obtaining UHPC concrete.
[0027] Example 2 A UHPC concrete comprises the following components in parts by weight: 35 parts of cement, 9 parts of silica fume, 13 parts of basalt fiber, 40 parts of quartz sand, 36 parts of modified garnet powder, 2 parts of sodium lignin sulfonate, 8 parts of water; The raw materials of the modified garnet powder include 30 parts of garnet powder and 6 parts of polyacrylonitrile with a weight average molecular weight of 50,000; The preparation method of modified garnet powder comprises the following steps: dissolving 6 parts of polyacrylonitrile with a weight average molecular weight of 50,000 in dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 8%, adding 30 parts of garnet powder to the polyacrylonitrile solution with a mass fraction of 8%, dispersing evenly, concentrating, and drying to obtain modified garnet powder; The preparation method of UHPC concrete comprises the following steps: stirring the remaining components except water and the water reducing agent at a stirring speed of 180 r / min for 13 minutes, blending, adding water and the water reducing agent, stirring at a stirring speed of 1300 r / min for 8 minutes, mixing evenly, and obtaining UHPC concrete.
[0028] Example 3 A UHPC concrete comprises the following components in parts by weight: 40 parts of cement, 10 parts of silica fume, 15 parts of basalt fiber, 65 parts of quartz sand, 40 parts of modified garnet powder, 3 parts of sodium lignin sulfonate, 10 parts of water; The raw materials of the modified garnet powder include 35 parts of garnet powder and 5 parts of polyacrylonitrile with a weight average molecular weight of 50,000; The preparation method of modified garnet powder comprises the following steps: dissolving 5 parts of polyacrylonitrile with a weight average molecular weight of 50,000 in dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 8%, adding 35 parts of garnet powder to the polyacrylonitrile solution with a mass fraction of 8%, dispersing evenly, concentrating, and drying to obtain modified garnet powder; The preparation method of UHPC concrete comprises the following steps: stirring the remaining components except water and water reducing agent at a stirring speed of 200 r / min for 10 minutes, blending, adding water and water reducing agent, stirring at a stirring speed of 1500 r / min for 5 minutes, mixing evenly, and obtaining UHPC concrete.
[0029] Example 4 The only difference between this embodiment and embodiment 2 is that in this embodiment, the raw materials of the modified garnet powder include 35 parts of garnet powder and 1 part of polyacrylonitrile with a weight average molecular weight of 50,000.
[0030] Example 5 The only difference between this embodiment and embodiment 2 is that in this embodiment, the raw materials of the modified garnet powder include 34 parts of garnet powder and 2 parts of polyacrylonitrile with a weight average molecular weight of 50,000.
[0031] Example 6 The only difference between this embodiment and embodiment 2 is that in this embodiment, the raw materials of the modified garnet powder include 32 parts of garnet powder and 4 parts of polyacrylonitrile with a weight average molecular weight of 50,000.
[0032] Example 7 The only difference between this embodiment and embodiment 6 is that in this embodiment, 4 parts of polyacrylonitrile with a weight average molecular weight of 50,000 are replaced by an equal amount of polyacrylonitrile with a weight average molecular weight of 150,000.
[0033] Example 8 The only difference between this embodiment and embodiment 6 is that in this embodiment, polyacrylonitrile is divided into first polyacrylonitrile and second polyacrylonitrile, the weight average molecular weight of the first polyacrylonitrile is 50,000, the weight average molecular weight of the second polyacrylonitrile is 150,000, 1 part of the first polyacrylonitrile is added, and 3 parts of the second polyacrylonitrile are added.
[0034] Example 9 The only difference between this embodiment and embodiment 8 is that, in this embodiment, 3.5 parts of the first polyacrylonitrile are added, and 0.5 parts of the second polyacrylonitrile are added.
[0035] Example 10 The only difference between this embodiment and embodiment 8 is that, in this embodiment, 2 parts of the first polyacrylonitrile are added, and 2 parts of the second polyacrylonitrile are added.
[0036] Embodiment 11 The only difference between this embodiment and embodiment 8 is that, in this embodiment, 3 parts of the first polyacrylonitrile are added, and 1 part of the second polyacrylonitrile is added.
[0037] Example 12 The difference between this embodiment and embodiment 10 is that, in this embodiment, the raw materials of the modified garnet powder include 27 parts of garnet powder, 4.5 parts of polyacrylonitrile (the weight ratio of the first polyacrylonitrile to the second polyacrylonitrile is 1:1) and 4.5 parts of o-hydroxybenzamide; The preparation method of modified garnet powder comprises the following steps: A1. Dissolve 4.5 parts of polyacrylonitrile in dimethylformamide to obtain a 6% polyacrylonitrile solution by mass, add 27 parts of garnet powder to the 6% polyacrylonitrile solution by mass, disperse evenly, concentrate, and dry to obtain a mixture; A2. Dissolve 4.5 parts of o-hydroxybenzamide in ethanol to obtain an o-hydroxybenzamide solution with a mass fraction of 8%. Add the mixture to the o-hydroxybenzamide solution with a mass fraction of 8%, disperse evenly, concentrate, and dry to obtain modified garnet powder.
[0038] Embodiment 13 The only difference between this embodiment and embodiment 12 is that in this embodiment, the raw materials of the modified garnet powder include 34 parts of garnet powder, 1 part of polyacrylonitrile (the weight ratio of the first polyacrylonitrile to the second polyacrylonitrile is 1:1) and 1 part of o-hydroxybenzamide.
[0039] Embodiment 14 The only difference between this embodiment and embodiment 12 is that in this embodiment, the raw materials of the modified garnet powder include 28 parts of garnet powder, 4 parts of polyacrylonitrile (the weight ratio of the first polyacrylonitrile to the second polyacrylonitrile is 1:1) and 4 parts of o-hydroxybenzamide.
[0040] Embodiment 15 The only difference between this embodiment and embodiment 12 is that in this embodiment, the raw materials of the modified garnet powder include 32 parts of garnet powder, 2 parts of polyacrylonitrile (the weight ratio of the first polyacrylonitrile to the second polyacrylonitrile is 1:1) and 2 parts of o-hydroxybenzamide.
[0041] Comparative Example 1 The only difference between this comparative example and Example 1 is that in this comparative example, 28 parts of modified garnet powder are replaced by an equal amount of garnet powder.
[0042] Comparative Example 2 The only difference between this comparative example and Example 1 is that in this comparative example, the raw materials of the modified garnet powder include 24 parts of garnet powder and 4 parts of styrene-acrylonitrile copolymer.
[0043] The UHPC concrete prepared in Examples 1 to 15 and Comparative Examples 1 to 2 was cured according to the curing method of the specimens in GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", and the curing age was 28 days. The following performance tests were performed on the cured concrete: Compressive strength: The compressive strength of UHPC concrete specimens was tested according to the test method of GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". The UHPC concrete specimen was a cubic specimen with a side length of 150 mm. During the test, the loading speed was 1.0 MPa / s.
[0044] Flexural strength: The flexural strength of the UHPC concrete specimens was tested according to the test method of GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". The UHPC concrete specimens were prismatic specimens with a side length of 150mm×150mm×600mm. During the test, the loading speed was 0.08MPa / s.
[0045] The test results are shown in Table 1 below: Table 1 Test results
[0046] Compared with Comparative Examples 1 and 2, the compressive strength and flexural strength of the UHPC concrete prepared in Example 1 are significantly improved, indicating that the compressive strength and flexural strength of the UHPC concrete can be improved by modifying the garnet powder with polyacrylonitrile.
[0047] Compared with Examples 2 and 4, the compressive strength and flexural strength of the UHPC concrete prepared in Examples 5 to 6 are improved, indicating that when the weight ratio of garnet powder to polyacrylonitrile is 8 to 17:1, it is helpful to further improve the compressive strength and flexural strength of the UHPC concrete. Compared with Examples 6 to 7, the compressive strength and flexural strength of the UHPC concrete prepared in Examples 8 to 11 are improved, indicating that the compressive strength and flexural strength of the UHPC concrete can be further improved by using the first polyacrylonitrile and the second polyacrylonitrile with different weight average molecular weights. Compared with Examples 8 to 9, the compressive strength and flexural strength of the UHPC concrete prepared in Examples 10 to 11 are improved, indicating that when the weight ratio of the first polyacrylonitrile to the second polyacrylonitrile is 1 to 3:1, the compressive strength and flexural strength of the UHPC concrete can be further improved. Compared with Example 10, the compressive strength and flexural strength of the UHPC concrete prepared in Examples 12 to 15 are improved, indicating that the use of polyacrylonitrile and o-hydroxybenzamide to modify garnet powder together can further improve the compressive strength and flexural strength of UHPC concrete. In addition, compared with Examples 12 to 13, the compressive strength and flexural strength of the UHPC concrete prepared in Examples 14 to 15 are improved, indicating that when the weight ratio of garnet powder, polyacrylonitrile and o-hydroxybenzamide is 7 to 16:1:1, it is helpful to further improve the compressive strength and flexural strength of UHPC concrete.
[0048] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A UHPC concrete, characterized in that: The composition comprises the following components in parts by weight: 30-40 parts of cement, 8-10 parts of silica fume, 10-15 parts of basalt fiber, 35-65 parts of quartz sand, 28-40 parts of modified garnet powder, 1-3 parts of water reducer, 6-10 parts of water; The raw materials of the modified garnet powder include garnet powder and polyacrylonitrile.
2. A UHPC concrete according to claim 1, characterized in that: The weight ratio of the garnet powder to the polyacrylonitrile is 8-17:
1.
3. A UHPC concrete according to claim 1, characterized in that: The preparation method of the modified garnet powder comprises the following steps: dissolving the polyacrylonitrile in dimethylformamide to obtain a polyacrylonitrile solution, adding the garnet powder into the polyacrylonitrile solution, dispersing evenly, concentrating, and drying to obtain the modified garnet powder.
4. The UHPC concrete according to claim 1, characterized in that: The polyacrylonitrile includes a first polyacrylonitrile and a second polyacrylonitrile, the weight average molecular weight of the first polyacrylonitrile is 50,000, and the weight average molecular weight of the second polyacrylonitrile is 150,000.
5. A UHPC concrete according to claim 4, characterized in that: The weight ratio of the first polyacrylonitrile to the second polyacrylonitrile is 1-3:
1.
6. The UHPC concrete according to claim 1, characterized in that: The raw material of the modified garnet powder also includes o-hydroxybenzamide.
7. A UHPC concrete according to claim 6, characterized in that: The weight ratio of the garnet powder, polyacrylonitrile and o-hydroxybenzamide is 7-16:1:
1.
8. The UHPC concrete according to claim 6, characterized in that: The preparation method of the modified garnet powder comprises the following steps: A1, dissolving the polyacrylonitrile in dimethylformamide to obtain a polyacrylonitrile solution, adding the garnet powder to the polyacrylonitrile solution, dispersing the mixture evenly, concentrating the mixture, and drying the mixture to obtain a mixture; A2, dissolving the o-hydroxybenzamide in ethanol to obtain an o-hydroxybenzamide solution, adding the mixture to the o-hydroxybenzamide solution, dispersing evenly, concentrating, and drying to obtain modified garnet powder.
9. The UHPC concrete according to claim 1, characterized in that: The water reducer is one or both of sodium lignin sulfonate and polycarboxylic acid water reducer.
10. A method for preparing UHPC concrete according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: blending the remaining components except water and the water reducing agent, adding water and the water reducing agent, mixing evenly, and obtaining UHPC concrete.