Red-layer soft rock roadbed mixture based on potassium fixation and strong cementation synergistic effect and preparation method of red-layer soft rock roadbed mixture
By using a modifier with synergistic effect of potassium fixation and strong cementation in the red layer soft rock subgrade mixture, its compressive strength and water stability are improved, and the low strength of the red layer soft rock subgrade mixture and easy water expansion and collapse The problem solved is applicable to the construction of highways in the red layer soft rock area, achieving resource utilization and economic benefits.
Patent Information
- Application Number
- CN202410901651.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-08
AI Technical Summary
As a roadbed filler, red layer soft rock has problems of low compressive strength and poor water stability, resulting in road settlement and high engineering construction and maintenance costs. Moreover, traditional gelling materials cannot be used for road construction on a large scale after improvement.
The preparation method of red layer soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation is used, using potassium humate and potassium formate as the first modifier, and ore powder, tricalcium silicate, calcium aluminate and calcium sulfate as The second modifier improves the compressive strength and water stability of the red layer soft rock through specific formula ratios and process steps.
It significantly improves the compressive strength and water stability of the red-layer soft rock roadbed mixture, is suitable for highway construction in red-layer soft rock area, realizes resource utilization, and has good environmental protection and economic benefits.
Abstract
Description
Technical Field
[0001] The invention relates to a technology for producing improved soil, in particular to a technology for producing a red layer soft rock roadbed mixture. Background Art
[0002] Red bed soft rock is a clastic rock sedimentary stratum formed after geological tectonic movement. Due to its special engineering properties, it has become a typical slippery stratum with characteristics such as easy weathering, cracking, water absorption, swelling and disintegration. It is a poor quality soil that needs to be properly disposed and utilized. There are a large number of red bed soft rock sections in the construction of expressways in central and western my country. This type of rock is mainly composed of minerals such as montmorillonite and illite, and most of them are disintegrating. When used for roadbed, it has poor physical properties such as high natural water content, high liquid limit and poor water stability. As a special roadbed filler, it often causes road settlement to varying degrees, increasing the cost of engineering construction and maintenance.
[0003] Traditional cementitious materials represented by cement are mixed with red soft rock to prepare roadbed mixtures. Although the cementitious properties of cement hydration can improve the compressive strength of red soft rock roadbed mixtures and offset the water absorption, expansion and cracking effect of red soft rock to a certain extent, it does not change the water absorption capacity of red soft rock in essence, resulting in the compressive strength of red soft rock roadbed mixtures being improved, but the water stability is still poor, and it cannot be used on a large scale for road construction. Therefore, by improving the red soft rock, reducing its water absorption capacity and improving its physical and mechanical properties, the improved red soft rock can be included in the category of roadbed fillings, which can not only reduce the cost of roadbed construction and reduce abandoned land, but also promote environmental protection, thereby bringing great economic benefits and ecological construction effects. Therefore, it is of urgent practical significance to develop a red soft rock roadbed mixture that specifically solves the above problems. Summary of the invention
[0004] In order to improve the compressive strength and water stability of a red-bed soft rock roadbed mixture, the present invention provides a red-bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation and a preparation method thereof.
[0005] The technical scheme adopted by the present invention is: a preparation method of a red-bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation, and the production raw material formula includes the following components in the following mass proportions: 100 parts of red-bed soft rock, 6 to 9 parts of a modifier; the modifier includes a first modifier and a second modifier, and the mass ratio of the first modifier to the second modifier is 1:6 to 16; the first modifier is composed of potassium humate and potassium formate in a mass ratio of 2 to 4:1; the second modifier is composed of the following components in the following mass proportions: 35 to 45 parts of mineral powder, 30 to 40 parts of tricalcium silicate, 2 to 5 parts of calcium aluminate, 12 to 15 parts of calcium sulfate, and 8 to 12 parts of anhydrous magnesium sulfate.
[0006] As a further improvement of the present invention, the particle size of the red bed soft rock is ≤1.18 mm and the water content is ≤5%.
[0007] As a further improvement of the present invention, the mineral powder is S95 grade mineral powder.
[0008] As a further improvement of the present invention, the mass percentage content of soluble humic acid in the potassium humate is ≥ 60% and K 2 The mass percentage content of O is ≥12%.
[0009] The preparation method of the present invention can be specifically implemented according to the following steps:
[0010] S1, measuring each raw material according to the production raw material formula;
[0011] S2. Reduce the water content of the red bed soft rock to ≤5%, crush it into particles and pass it through a 1.18 mm square hole sieve. The sieved material is the pre-treated red bed soft rock; and then determine the total amount of water added according to the standard test method;
[0012] S3, mixing the pretreated red bed soft rock and the first modifier evenly, then adding water according to 1 / 2 of the total amount of water, mixing evenly again, and bagging, sealing and stuffing at room temperature for 18 to 24 hours to obtain modified slurry;
[0013] S4, adding water according to 1 / 2 of the total amount of water added to the second modifier and stirring evenly to obtain a second modifier slurry;
[0014] S5. Add the modified slurry into the second modifier slurry at a uniform speed, control the stirring rate to 200-300 r / min during the adding process, and continue stirring for 5-6 minutes to obtain.
[0015] Those skilled in the art will understand that the above “determine the total amount of water added according to the standard test method” means to calculate the total amount of water added according to the standard test method of “Testing Procedure for Stabilized Materials of Inorganic Binders for Highway Engineering” JTG 3441-2024. If the procedure is revised, the revised corresponding procedure will naturally be used.
[0016] The present invention also discloses a red-layer soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation, which is prepared by the preparation method of the red-layer soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation of the present invention.
[0017] The beneficial effects of the present invention are as follows: the preparation method of the present invention can significantly improve the compressive strength and water stability of the red layer soft rock roadbed mixture, solve the engineering application problems of low strength of the red layer soft rock roadbed mixture and easy expansion and disintegration when exposed to water, is suitable for highway construction in red layer soft rock areas, achieves the purpose of resource utilization of red layer soft rock, and has good environmental protection and economic benefits. DETAILED DESCRIPTION
[0018] The present invention is further described below in conjunction with embodiments.
[0019] Embodiment 1:
[0020] The red layer soft rock roadbed mixture is prepared as follows:
[0021] (1) The raw materials are measured according to the following raw material formula: 100 parts of red bed soft rock (by dry weight), 7.7 parts of modifier; the modifier includes a first modifier and a second modifier, and the mass ratio of the first modifier to the second modifier is 1:10; the first modifier is potassium humate (the mass percentage content of soluble humic acid is 67.6%, K 2 O content of 14.8% by mass. ) and potassium formate in a mass ratio of 3:1; the second modifier is composed of the following components in mass proportions: 37.4 parts of mineral powder (S95 grade), 34.8 parts of tricalcium silicate, 3.6 parts of calcium aluminate, 13.8 parts of calcium sulfate, and 10.2 parts of anhydrous magnesium sulfate.
[0022] (2) The red layer soft rock is dried and the moisture content is measured to be 4.66%, then it is crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material is the pre-treated red layer soft rock; and the total amount of water added is determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG3441-2024;
[0023] (3) The pretreated red bed soft rock and the first modifier are mixed evenly, and then water is added according to 1 / 2 of the total amount of water, and the mixture is mixed evenly again, and then packed into a plastic bag, and sealed at room temperature for 22 hours to obtain a modified slurry;
[0024] (4) adding 1 / 2 of the total amount of water to the second modifier and stirring evenly to obtain a second modifier slurry;
[0025] (5) The modified slurry is added to the second modifier slurry at a uniform speed, and the stirring rate is controlled to be 300 r / min during the adding process and the stirring is continued for 5 minutes to obtain a red layer soft rock roadbed mixture.
[0026] Embodiment 2:
[0027] The red layer soft rock roadbed mixture is prepared as follows:
[0028] (1) The raw materials are measured according to the following raw material formula: 100 parts of red bed soft rock (by dry weight), 8.9 parts of modifier; the modifier includes a first modifier and a second modifier, and the mass ratio of the first modifier to the second modifier is 1:8.9; the first modifier is composed of potassium humate (the mass percentage content of soluble humic acid is 67.6%, K2 O content of 14.8% by mass. ) and potassium formate in a mass ratio of 2.7:1; the second modifier is composed of the following components in mass proportions: 35.1 parts of mineral powder (S95 grade), 37.2 parts of tricalcium silicate, 2.3 parts of calcium aluminate, 14.9 parts of calcium sulfate, and 11.6 parts of anhydrous magnesium sulfate.
[0029] (2) The red layer soft rock is dried and the moisture content is measured to be 4.38%, then it is crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material is the pre-treated red layer soft rock; and the total amount of water added is determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG3441-2024;
[0030] (3) The pretreated red bed soft rock and the first modifier are mixed evenly, and then water is added according to 1 / 2 of the total amount of water, and the mixture is mixed evenly again, and then packed into a plastic bag, and sealed at room temperature for 24 hours to obtain a modified slurry;
[0031] (4) adding 1 / 2 of the total amount of water to the second modifier and stirring evenly to obtain a second modifier slurry;
[0032] (5) The modified slurry is uniformly added to the second modifier slurry, and the stirring rate is controlled to be 250 r / min during the adding process and the stirring is continued for 5.5 min to obtain a red layer soft rock roadbed mixture.
[0033] Embodiment three:
[0034] The red layer soft rock roadbed mixture is prepared as follows:
[0035] (1) The raw materials are measured according to the following raw material formula: 100 parts of red bed soft rock (by dry weight), 6.8 parts of modifier; the modifier includes a first modifier and a second modifier, and the mass ratio of the first modifier to the second modifier is 1:7.5; the first modifier is composed of potassium humate (the mass percentage content of soluble humic acid is 67.6%, K 2 O content of 14.8% by mass. ) and potassium formate in a mass ratio of 3.5:1; the second modifier is composed of the following components in mass proportions: 42.6 parts of mineral powder (S95 grade), 33.4 parts of tricalcium silicate, 3.5 parts of calcium aluminate, 12.4 parts of calcium sulfate, and 8.7 parts of anhydrous magnesium sulfate.
[0036] (2) The red layer soft rock is dried and the moisture content is measured to be 4.35%, then it is crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material is the pre-treated red layer soft rock; and the total amount of water added is determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG3441-2024;
[0037] (3) The pretreated red bed soft rock and the first modifier are mixed evenly, and then water is added according to 1 / 2 of the total amount of water, and the mixture is mixed evenly again, and then packed into a plastic bag, and sealed at room temperature for 19 hours to obtain a modified slurry;
[0038] (4) adding 1 / 2 of the total amount of water to the second modifier and stirring evenly to obtain a second modifier slurry;
[0039] (5) The modified slurry is added to the second modifier slurry at a uniform speed, and the stirring rate is controlled to be 220 r / min during the adding process and the stirring is continued for 5.75 min to obtain a red layer soft rock roadbed mixture.
[0040] Comparative Example 1:
[0041] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as the example, and the raw materials used are from the same batch as Example 1, except that no modifier is used. The specific implementation is as follows:
[0042] (1) Measure the raw materials according to the following production raw material formula: 100 parts of red bed soft rock (by dry weight);
[0043] (2) The red layer soft rock was dried and the moisture content was measured to be 4.66%, and then it was crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material was the pre-treated red layer soft rock (the same batch as in Example 1); and the total amount of water added was determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG 3441-2024;
[0044] (3) adding water according to 1 / 2 of the total amount of water to the pretreated red layer soft rock, mixing evenly, and then putting it into a plastic bag, sealing and stuffing the material at room temperature for 22 hours to obtain a modified slurry;
[0045] (4) The modified slurry is uniformly added to the remaining 1 / 2 amount of water. During the adding process, the stirring rate is controlled to be 300 r / min and the stirring is continued for 5 minutes to obtain a red layer soft rock roadbed mixture.
[0046] Comparative Example 2:
[0047] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as Example 1. The raw materials used are from the same batch as Example 1, and the difference is that the modifier is replaced by ordinary Portland cement of the same mass. The specific implementation is as follows:
[0048] (1) Measure the raw materials according to the following production raw material formula: 100 parts of red bed soft rock (by dry weight), 7.7 parts of Portland cement;
[0049] (2) The red layer soft rock was dried and the moisture content was measured to be 4.66%, and then it was crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material was the pre-treated red layer soft rock (the same batch as in Example 1); and the total amount of water added was determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG 3441-2024;
[0050] (3) The pretreated red bed soft rock was mixed evenly with 0.7 parts of ordinary Portland cement, and then 1 / 2 of the total amount of water was added and mixed evenly again, and then put into a plastic bag, and sealed at room temperature for 22 hours to obtain a modified slurry;
[0051] (4) adding 1 / 2 of the total amount of water to the remaining ordinary Portland cement and stirring evenly to obtain a slurry;
[0052] (5) The modified slurry is added to the slurry at a uniform speed, and the stirring rate is controlled to be 300 r / min during the adding process and the stirring is continued for 5 minutes to obtain a red layer soft rock roadbed mixture.
[0053] Comparative Example 3:
[0054] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as the example, and the raw materials used are from the same batch as Example 1, except that the first modifier is not used. The specific implementation is as follows:
[0055] (1) The raw materials are measured according to the following production raw material formula: 100 parts of red bed soft rock (by dry weight), 7 parts of the second modifier; the second modifier is composed of the following components in the following mass proportions: 37.4 parts of mineral powder (S95 grade), 34.8 parts of tricalcium silicate, 3.6 parts of calcium aluminate, 13.8 parts of calcium sulfate, and 10.2 parts of anhydrous magnesium sulfate.
[0056] (2) The red layer soft rock was dried and the moisture content was measured to be 4.66%, and then it was crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material was the pre-treated red layer soft rock (the same batch as in Example 1); and the total amount of water added was determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG 3441-2024;
[0057] (3) adding water according to 1 / 2 of the total amount of water to the pretreated red layer soft rock, mixing evenly, and then putting it into a plastic bag, sealing and stuffing the material at room temperature for 22 hours to obtain a modified slurry;
[0058] (4) adding 1 / 2 of the total amount of water to the second modifier and stirring evenly to obtain a second modifier slurry;
[0059] (5) The modified slurry is added to the second modifier slurry at a uniform speed, and the stirring rate is controlled to be 300 r / min during the adding process and the stirring is continued for 5 minutes to obtain a red layer soft rock roadbed mixture.
[0060] Comparative Example 4:
[0061] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as the example, and the raw materials used are from the same batch as Example 1, except that the second modifier is not used. The specific implementation is as follows:
[0062] (1) According to the following raw material formula, the raw materials are measured: 100 parts of red bed soft rock (by dry weight), 0.7 parts of the first modifier; the first modifier is composed of potassium humate (the mass percentage of soluble humic acid is 67.6%, K 2 The mass percentage content of O is 14.8%. ) and potassium formate are composed in a mass ratio of 3:1.
[0063] (2) The red layer soft rock was dried and the moisture content was measured to be 4.66%, and then it was crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material was the pre-treated red layer soft rock (the same batch as in Example 1); and the total amount of water added was determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG 3441-2024;
[0064] (3) The pretreated red bed soft rock and the first modifier are mixed evenly, and then water is added according to 1 / 2 of the total amount of water, and the mixture is mixed evenly again, and then packed into a plastic bag, and sealed at room temperature for 22 hours to obtain a modified slurry;
[0065] (4) The modified slurry is uniformly added to the remaining 1 / 2 amount of water. During the adding process, the stirring rate is controlled to be 300 r / min and the stirring is continued for 5 minutes to obtain a red layer soft rock roadbed mixture.
[0066] Comparative Example 5:
[0067] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as the example, and the raw materials used are from the same batch as Example 1, except that: the first modifier is all potassium humate (the total amount of the first modifier remains unchanged).
[0068] (1) The raw materials are measured according to the following raw material formula: 100 parts of red bed soft rock (by dry weight), 7.7 parts of modifier; the modifier includes a first modifier and a second modifier, and the mass ratio of the first modifier to the second modifier is 1:10; the first modifier is potassium humate (the mass percentage content of soluble humic acid is 67.6%, K 2The mass percentage content of O is 14.8%. ); The second modifier is composed of the following components in the following mass proportions: 37.4 parts of mineral powder (S95 grade), 34.8 parts of tricalcium silicate, 3.6 parts of calcium aluminate, 13.8 parts of calcium sulfate, and 10.2 parts of anhydrous magnesium sulfate.
[0069] (2) The red layer soft rock was dried and the moisture content was measured to be 4.66%, and then it was crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material was the pre-treated red layer soft rock (the same batch as in Example 1); and the total amount of water added was determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG 3441-2024;
[0070] (3) The pretreated red bed soft rock and the first modifier are mixed evenly, and then water is added according to 1 / 2 of the total amount of water, and the mixture is mixed evenly again, and then packed into a plastic bag, and sealed at room temperature for 22 hours to obtain a modified slurry;
[0071] (4) adding 1 / 2 of the total amount of water to the second modifier and stirring evenly to obtain a second modifier slurry;
[0072] (5) The modified slurry is added to the second modifier slurry at a uniform speed, and the stirring rate is controlled to be 300 r / min during the adding process and the stirring is continued for 5 minutes to obtain a red layer soft rock roadbed mixture.
[0073] Comparative Example 6:
[0074] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as the example, and the raw materials used are from the same batch as Example 1, with the difference that the first modifier is all potassium formate (the total amount of the first modifier remains unchanged).
[0075] (1) The raw materials are measured according to the following production raw material formula: 100 parts of red bed soft rock (by dry weight), 7.7 parts of modifier; the modifier includes a first modifier and a second modifier, and the mass ratio of the first modifier to the second modifier is 1:10; the first modifier is potassium formate; the second modifier is composed of the following components in the following mass proportions: 37.4 parts of mineral powder (S95 grade), 34.8 parts of tricalcium silicate, 3.6 parts of calcium aluminate, 13.8 parts of calcium sulfate, and 10.2 parts of anhydrous magnesium sulfate.
[0076] (2) The red layer soft rock was dried and the moisture content was measured to be 4.66%, and then it was crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material was the pre-treated red layer soft rock (the same batch as in Example 1); and the total amount of water added was determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG 3441-2024;
[0077] (3) The pretreated red bed soft rock and the first modifier are mixed evenly, and then water is added according to 1 / 2 of the total amount of water, and the mixture is mixed evenly again, and then packed into a plastic bag, and sealed at room temperature for 22 hours to obtain a modified slurry;
[0078] (4) adding 1 / 2 of the total amount of water to the second modifier and stirring evenly to obtain a second modifier slurry;
[0079] (5) The modified slurry is added to the second modifier slurry at a uniform speed, and the stirring rate is controlled to be 300 r / min during the adding process and the stirring is continued for 5 minutes to obtain a red layer soft rock roadbed mixture.
[0080] Comparative Example 7:
[0081] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as the example, and the raw materials used are from the same batch as Example 1, and the difference is that the order of adding the first modifier and the second modifier is exchanged. The specific steps are as follows:
[0082] (1) The raw materials are measured according to the following raw material formula: 100 parts of red bed soft rock (by dry weight), 7.7 parts of modifier; the modifier includes a first modifier and a second modifier, and the mass ratio of the first modifier to the second modifier is 1:10; the first modifier is potassium humate (the mass percentage content of soluble humic acid is 67.6%, K 2 O content of 14.8% by mass. ) and potassium formate in a mass ratio of 3:1; the second modifier is composed of the following components in mass proportions: 37.4 parts of mineral powder (S95 grade), 34.8 parts of tricalcium silicate, 3.6 parts of calcium aluminate, 13.8 parts of calcium sulfate, and 10.2 parts of anhydrous magnesium sulfate.
[0083] (2) The red layer soft rock was dried and the moisture content was measured to be 4.66%, and then it was crushed into particles and passed through a 1.18 mm square hole sieve. The sieved material was the pre-treated red layer soft rock (the same batch as in Example 1); and the total amount of water added was determined according to the standard test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG 3441-2024;
[0084] (3) adding 1 / 2 of the total amount of water to the second modifier and stirring evenly to obtain a second modifier slurry;
[0085] (4) The pretreated red bed soft rock is uniformly added to the second modifier slurry, the stirring rate is controlled to be 300 r / min during the adding process, and the stirring is continued for 5 minutes to obtain a modified slurry.
[0086] (5) The modified slurry and the first modifier are mixed evenly, and then water is added according to 1 / 2 of the total amount of water, and the mixture is mixed evenly again, and then the mixture is packed into a plastic bag, and the mixture is sealed at room temperature for 22 hours to obtain a red layer soft rock roadbed mixture.
[0087] Red layer soft rock roadbed mixture performance test:
[0088] The red layer soft rock roadbed mixtures prepared in the above embodiments and comparative examples were taken, and the static pressing compaction degree was fixed to 96%. According to the "Test Procedure for Stabilized Materials of Inorganic Binders for Highway Engineering" JTG3441-2024 and the "Technical Standard for the Application of Soil Solidifiers" CJJ / T286-2018, the 7d unconfined compressive strength and water stability coefficient of the red layer soft rock roadbed mixture samples in the embodiments and comparative examples were respectively measured. The measurement results are shown in Table 1.
[0089] Table 1 Test results of compressive strength and water stability coefficient of red soft rock roadbed mixture
[0090] serial number 7d unconfined compressive strength / MPa Water stability coefficient / % Embodiment 1 5.48 107.7 Embodiment 2 5.12 95.6 Embodiment 3 4.77 96.7 Comparative Example 1 (blank control) 0 0 Comparative Example 2 (Portland Cement) 3.69 78.2 Comparative Example 3 (single second modifier) 3.81 86.8 Comparative Example 4 (single first modifier) 0 0 Comparative Example 5 (Potassium monohumate) 4.25 92.9 Comparative Example 6 (Potassium Monoformate) 4.51 98.4 Comparative Example 7 (changing the order of modifiers) 1.65 43.3
[0091] It can be seen from the test results of Example 1, Example 2 and Example 3 in Table 1 that the 7d unconfined compressive strength of the red layer soft rock roadbed mixture prepared by the method of the present invention can reach more than 4.77MPa, and the water stability coefficient can reach more than 95.6%, which has excellent strength and water stability.
[0092] From the comparison between Example 1 and Comparative Example 1 in Table 1, it can be seen that the 7d unconfined compressive strength and water stability coefficient of the blank control group without using any modifier are both 0, and the 7d unconfined compressive strength and water stability coefficient of the red layer soft rock roadbed mixture prepared using the modifier and preparation method of the present invention are 5.48MPa and 107.7%, respectively. It can be seen that the modifier of the present invention has a very significant technical effect of improving the compressive strength and water stability of the red layer soft rock roadbed mixture.
[0093] From the comparison of Example 1, Comparative Example 1 and Comparative Example 2 in Table 1, it can be seen that although the addition of silicate cement can improve the compressive strength of the red layer soft rock roadbed mixture to a certain extent, the water stability coefficient still does not meet the standard use requirements. The reason is that the bonding performance of silicate cement hydration can improve the compressive strength of the red layer soft rock roadbed mixture, which offsets the water absorption, expansion and cracking effect of the red layer soft rock to a certain extent, but does not essentially change the water absorption capacity of the red layer soft rock, resulting in the compressive strength of the red layer soft rock roadbed mixture being improved but the water stability is still not high.
[0094] From the comparison of Example 1, Comparative Example 3 and Comparative Example 4 in Table 1, it can be seen that when the second modifier is used alone, the compressive strength and water stability coefficient of the red layer soft rock roadbed mixture are 3.81Mpa and 86.8% respectively; while when the first modifier is used alone, the compressive strength and water stability coefficient are both 0. Through calculation, it can be known that theoretically, when the two are used in combination, the compressive strength and water stability coefficient of the red layer soft rock roadbed mixture should be 3.81Mpa and 86.8% respectively, while the actual measured values are 5.48Mpa and 107.7%, which are significantly higher than the theoretical values of 43.8% and 24.1% respectively. It can be seen that the first modifier and the second modifier have a significant synergistic effect in improving the compressive strength and water stability of the red layer soft rock roadbed mixture when used in combination.
[0095] From the comparison of Example 1, Comparative Example 3, Comparative Example 5 and Comparative Example 6 in Table 1, it can be seen that the compressive strength and water stability coefficient of the red layer soft rock roadbed mixture of Comparative Example 5, which uses potassium humate alone on the basis of Comparative Example 3, are increased by 0.44Mpa and 6.1% respectively; while the corresponding values when potassium formate is used alone are increased by 0.70Mpa and 11.6% respectively. Through calculation, it can be known that under the premise of the unchanged amount of the first modifier, after potassium humate and potassium formate are mixed in a mass ratio of 3:1, the theoretical compressive strength and water stability coefficient of the red layer soft rock roadbed mixture should be 4.32Mpa and 94.3% respectively, while the actual measured values are 5.48Mpa and 107.7%, which are significantly higher than the theoretical values of 26.9% and 14.2%, respectively. It can be seen that potassium humate and potassium formate have a significant synergistic effect in improving the compressive strength and water stability of the red layer soft rock roadbed mixture.
[0096] From the comparison between Example 1 and Comparative Example 7 in Table 1, it can be seen that when the order of adding the modifiers is changed, the compressive strength and water stability coefficient of the red layer soft rock roadbed mixture are 1.65 MPa and 43.3%, respectively, which are significantly reduced compared with Example 1.
Claims
1. A method for preparing a red-bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation, characterized in that: The production raw material formula includes the following components in proportion by mass: 100 parts of red bed soft rock and 6 to 9 parts of modifier; the modifier includes a first modifier and a second modifier, and the mass ratio of the first modifier to the second modifier is 1:6 to 16; the first modifier is composed of potassium humate and potassium formate in a mass ratio of 2 to 4:1; the second modifier is composed of the following components in proportion by mass: 35 to 45 parts of mineral powder, 30 to 40 parts of tricalcium silicate, 2 to 5 parts of calcium aluminate, 12 to 15 parts of calcium sulfate, and 8 to 12 parts of anhydrous magnesium sulfate.
2. The method for preparing a red bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation according to claim 1, characterized in that: The particle size of the red bed soft rock is ≤1.18 mm, and the water content is ≤5%.
3. The method for preparing a red bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation according to claim 1, characterized in that: The mineral powder is S95 grade mineral powder.
4. The method for preparing a red bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation according to claim 1, characterized in that: The mass percentage content of soluble humic acid in the potassium humate is ≥60%, and the mass percentage content of K2O is ≥12%.
5. The method for preparing a red bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation according to any one of claims 1 to 4, characterized in that: The steps include: S1, measuring each raw material according to the production raw material formula; S2. Reduce the water content of the red bed soft rock to ≤5%, crush it into particles and pass it through a 1.18 mm square hole sieve. The sieved material is the pre-treated red bed soft rock; and then determine the total amount of water added according to the standard test method; S3, mixing the pretreated red bed soft rock and the first modifier evenly, then adding water according to 1 / 2 of the total amount of water, mixing evenly again, and bagging, sealing and stuffing at room temperature for 18 to 24 hours to obtain modified slurry; S4, adding water according to 1 / 2 of the total amount of water added to the second modifier and stirring evenly to obtain a second modifier slurry; S5. Add the modified slurry into the second modifier slurry at a uniform speed, control the stirring rate to 200-300 r / min during the adding process, and continue stirring for 5-6 minutes to obtain.
6. A red bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation, obtained by the preparation method of the red bed soft rock roadbed mixture based on the synergistic effect of potassium fixation and strong cementation as described in any one of claims 1 to 5.