High-strength solidified soil, solidified soil road surface layer and construction technology of solidified soil road surface layer
By combining curing agents such as cement, sodium silicate and calcium carbonate with raw materials such as yellow mud and bean gravel, the compressive strength and compactness of the cured soil are improved, and a protective layer is set up in the road surface layer to solve the pressure resistance of the cured soil. The problems of insufficient strength and complex construction have achieved efficient and economical road surface construction.
Patent Information
- Application Number
- CN202410982178.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The compressive strength of the existing solidified soil is less than 5MPa and cannot be used as a road surface layer alone. In some urban roads, garden scenic spots, modern agriculture and animal husbandry, ecological construction and other projects, due to the construction pollution and materials of asphalt concrete and cement concrete surface layer. It is difficult to supply, the road surface is expensive and the construction process is cumbersome, making it difficult to adopt.
Use cement, sodium silicate and calcium carbonate as curing agents to form calcium silicate gel and carbonate through chemical reactions to improve the soil's permeability and durability, and combine raw materials such as yellow mud, bean gravel, fine sand, etc. High-strength cured soil is prepared by dry mixing or fluid mixing to increase the compactness and bearing capacity of the soil; a waste brick particle base layer and a high-strength cured soil layer are installed in the road surface layer, and protective liquid and resistance are sprayed on the high-strength cured soil layer Abrasives form a dense and impermeable film, enhancing waterproof and impermeable resistance and wear resistance.
Improve the compressive strength and compactness of the solidified soil, simplify the construction process, reduce costs, and form a road surface layer with strong crack resistance, high compressive strength, good seepage effect and wear resistance. It is suitable for a variety of projects environment.
Smart Images

Figure BDA0004956398050000081 
Figure BDA0004956398050000091 
Figure BDA0004956398050000092
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of civil engineering materials, and more specifically, to a high-strength solidified soil, a solidified soil road surface layer and a construction process thereof. Background Art
[0002] Solidified soil (stabilized soil) is a geotechnical engineering material. With the application of soil stabilizers, the physical and mechanical properties of solidified soil have been improved, making solidified soil a new geotechnical engineering material. It has been used in road construction, beach reclamation, river and lake management, water conservancy projects, farmland construction and many other aspects. For example, in road construction, traditional process methods require the use of a large amount of sand and gravel. However, with the development of my country's construction and the requirements of environmental protection, many areas have opened mountains to obtain stones, and the contradiction between sand and gravel production and the environment has become increasingly prominent. The supply of sand and gravel has become increasingly difficult, and the construction cost has been greatly increased. The use of solidified soil technology and the use of solidified soil as the road base can make full use of the original soil without or with less sand and gravel. Not only is the construction convenient and the project quality improved, but it also saves resources and reduces project costs.
[0003] The existing solidified soil generally has low strength, with a compressive strength of less than 5MPa. In road construction, it can only be used as a base layer. Its surface layer still uses traditional asphalt concrete or cement concrete. However, in the construction of solidified soil roads in some urban roads, garden scenic spots, modern agriculture and animal husbandry, ecological construction and other projects, due to many problems such as pollution during construction of asphalt concrete and cement concrete surface layers, difficulty in material supply, high road construction cost, and complicated construction process, it is sometimes difficult to use. It is necessary to find a new light-load road surface material. Directly using solidified soil as a road surface has low strength and cannot be used as a road surface alone.
[0004] In view of the above-mentioned related technologies, there is an urgent need for a solidified soil with high strength that can be used alone as a road surface layer. Summary of the invention
[0005] In order to improve the density and strength of solidified soil, the present application provides a high-strength solidified soil, a preparation method thereof, and a solidified soil road surface layer.
[0006] In the first aspect, the present application provides a high-strength solidified soil, which adopts the following technical solution: A high-strength solidified soil comprises the following raw materials in parts by weight: 300-1000 parts of a solidifying agent, 0-600 parts of fine sand, 300-3500 parts of yellow mud, 0-500 parts of pea gravel, and 250-500 parts of water. The solidifying agent comprises cement, sodium silicate, and calcium carbonate in a mass ratio of 7-8:1-1.5:1-1.5.
[0007] By adopting the above technical solution, cement, sodium silicate and calcium carbonate are used as curing agents. Sodium silicate has good penetration ability and can quickly penetrate into the solidified soil to react chemically with free calcium ions and magnesium ions in the soil. Moreover, the sodium ions in sodium silicate can undergo ion exchange reaction with free calcium and magnesium ions in the soil to form a stable calcium silicate gel, which fixes the soil particles in the soil and improves the soil's impermeability and durability. Calcium carbonate mainly combines with heavy metal ions in the soil through calcium carbonate ions to form insoluble carbonates, thereby reducing the flow of heavy metals in the soil. It solidifies the soil and improves the soil's pH and structure. Cement can react with water in the mud to generate various hydrates, and undergo a series of physical and chemical reactions with soil particles to improve the soil's engineering properties. Specifically, tricalcium silicate, dicalcium silicate and other minerals in cement react with water to generate hydrates such as calcium hydroxide and hydrated calcium silicate. These hydrates form tiny crystals in the soil, filling the gaps between soil particles, enhancing the bonding force between particles, making the soil denser, and thus improving the soil's overall strength, impermeability, bearing capacity and stability.
[0008] Optionally, the high-strength solidified soil comprises the following raw materials in parts by weight: 950-1000 parts of a curing agent, 3450-3500 parts of Yellow mud, 450-500 parts of water, and the curing agent comprises cement, sodium silicate and calcium carbonate in a mass ratio of 8:1:1.
[0009] By adopting the above technical scheme, yellow mud, water and a curing agent are mixed to prepare dry-mixed solidified soil, and the obtained solidified soil has high compressive strength and high density.
[0010] Optionally, the high-strength solidified soil comprises the following raw materials in parts by weight: 300-400 parts of a curing agent, 550-600 parts of fine sand, 300-350 parts of yellow mud, 350-500 parts of pea gravel, and 250-300 parts of water, wherein the curing agent comprises cement, sodium silicate, and calcium carbonate in a mass ratio of 8:1:1.
[0011] By adopting the above technical solution, fine sand, pea gravel, curing agent and yellow mud are mixed to form fluidized solidified soil, which has high strength and good impermeability after curing.
[0012] Optionally, the particle size of the pea gravel is 1-2 cm.
[0013] By adopting the above technical scheme, pea gravel is used as coarse aggregate and as a supporting structure in the solidified soil, and cooperates with fine sand to improve the strength of the solidified soil. If the pea gravel particle size is small and the grading is poor, more fine sand and yellow mud are needed to fill the gaps, resulting in low flexural strength. As the particle size increases, the grading becomes more reasonable, so that there are fewer weak links in the interface, which improves the flexural strength of the solidified soil. If the particle size increases further, there are fewer bonding interfaces, and the bonding interfaces between pea gravel and yellow mud, cement, etc. are weak links in strength development, the concrete is prone to stress concentration failure, and the flexural strength begins to decrease again.
[0014] Optionally, the pea gravel is pretreated as follows: carbide slag, rice husk ash and water are mixed evenly in a ratio of 1.8-2:1:1.4-1.5 to prepare a slurry; Add pea gravel to the slurry, stir thoroughly, then place the pea gravel coated with slurry on a wire mesh and let it stand for 2-3 hours, then maintain constant temperature and humidity for 28 days to obtain aggregate; Mix epoxy resin and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane in a mass ratio of 10:0.8-1, add aggregate, stir thoroughly, spread evenly and let stand for 20-24 hours.
[0015] By adopting the above technical scheme, both carbide slag and rice husk ash are solid waste materials. Using the two to improve the strength of pea gravel has significant economic benefits; the chemical composition of carbide slag is mainly calcium oxide, and the main minerals are calcium hydroxide and calcite. Rice husk ash is made by burning rice husks in a diluted oxygen environment of 500-800℃, contains a large amount of free silicon dioxide, has high volcanic ash activity, and can be used as a component of cementitious materials; after the two are mixed, the calcium hydroxide in the carbide slag and the silicon dioxide in the rice husk ash are in the water environment. The reaction forms CSH gel, so after the pea gravel is fully stirred in the slurry, the slurry is wrapped on the pea gravel, reducing the porosity of the pea gravel and increasing the density. After hydration and hardening, a coating layer with high bonding strength and good mechanical properties is formed on the surface of the pea gravel, thereby improving the bearing capacity of the pea gravel and making it less prone to wear and breakage; then the epoxy resin and curing agent are mixed and coated on the aggregate. The epoxy resin has good hydrophobicity and can reduce the water absorption and hygroscopicity of the pea gravel, thereby improving the moisture permeability of the solidified soil and improving the anti-seepage ability.
[0016] In the second aspect, the present application provides a method for preparing a cured earth road pavement, adopting the following technical scheme: a cured earth road pavement, comprising a base layer containing waste brick particles and a high-strength cured earth layer located above the base layer, wherein the high-strength cured earth layer is formed by laying and rolling high-strength cured earth on the base layer.
[0017] By adopting the above technical scheme, a base layer containing waste brick particles is used as a primer, and high-strength solidified soil is laid on the base layer. After rolling, high-strength solidified soil is formed, which has high strength, simple construction method and low cost.
[0018] Optionally, the cured soil road surface layer also includes a protective layer located above the high-strength cured soil layer, and the protective layer includes 4-8 parts by weight of silicone emulsion and 0.3-0.5 parts by weight of wear resistance agent, 0.01-0.02 parts by weight of defoaming agent, 0.02-0.04 parts by weight of hydrogenated silicone oil, 0.1-0.5 parts by weight of silicon dioxide, and 1-2 parts by weight of water.
[0019] By adopting the above technical scheme, high-strength solidified soil is easy to get dusty on sunny days, slippery on rainy days, and has insufficient wear resistance. A protective layer is set on the high-strength solidified soil layer, and the silicone emulsion acts on the soil particles in the high-strength solidified soil at a certain thickness of the protective layer, so that the soil particles are adsorbed and superimposed to form a dense and impermeable film, which reduces the infiltration capacity of water in the soil, enhances the waterproof and anti-seepage capacity of the road surface, and reduces the dusting phenomenon of the high-strength solidified soil layer. The wear-resistant agent and silica can increase the wet friction of the road surface layer and increase the wear resistance.
[0020] Optionally, the method for preparing the wear-resistant agent comprises the following steps: In parts by weight, 2-5 parts of clay, 0.5-1.5 parts of fly ash and 1.5-3 parts of water are mixed, and 0.04-0.1 parts of calcium lignin sulfonate are added, and the mixture is granulated, dried, and ball-milled to obtain spherical bodies with a particle size of 100-150 μm; The spherical body is mixed with 0.09-0.1 parts of polyvinyl alcohol, 2.5-6.5 parts of polyimide and 30-40 parts of water to form a mixed slurry; the mixed slurry is spray granulated, dried and sintered to obtain a wear-resistant agent, the spray drying inlet temperature is 110-115°C, the outlet temperature is 130-135°C, and the flow rate is 60-65ml / min.
[0021] By adopting the above technical scheme, fly ash, as an industrial waste, has a huge annual emission volume, which has caused great pressure on the ecological environment. Fly ash is mainly composed of oxides of silicon, aluminum and calcium, with a large specific surface area, stable composition and certain or. Therefore, when mixed with clay and water, it can increase the gelation of clay to form a hard sphere. In addition, due to the addition of calcium lignin sulfonate, the strength and impermeability of the sphere can be improved. Calcium lignin sulfonate can rearrange clay and fly ash particles through dispersion and bridging, and also has the function of filling pores. In addition, through the chemical chain effect formed by its hydrophilic group and the metal cations on the surface of the clay particles, lignin is adsorbed on the surface of the clay particles, and the hydrophobic group forms an oily layer around the surface of the clay particles. It has a certain exclusion effect on the water on the surface of clay particles and prevents moisture from entering; the addition of calcium lignin sulfonate can also improve the dispersion uniformity of spherical bodies, polyimide and polyvinyl alcohol. When spray granulation is performed, polyvinyl alcohol is used as a binder. The mixed slurry forms a high-speed liquid film during the atomization process and splits into droplets. Due to the effect of surface tension, the droplets gradually form spheres, evaporate and dry quickly, and are finally coated on the surface of the spheres to obtain a granular wear-resistant agent. The coating of polyimide can improve the dispersibility of the spheres in the silicone emulsion, thereby making the wear-resistant agent evenly distributed in the protective layer. In addition, polyimide has high mechanical strength, high temperature resistance and chemical stability, and has good wear resistance, so the wear-resistant agent prepared can effectively improve the wear resistance of the road surface.
[0022] Optionally, the high-strength solidified soil layer has a thickness of 10-15 cm, and the protective layer has a thickness of 10-15 mm.
[0023] By adopting the above technical solution, the protective layer is arranged on the high-strength solidified soil layer, which can prevent dusting and increase the wear resistance of the high-strength solidified soil layer.
[0024] In a third aspect, the present application provides a construction process for a solidified soil road surface layer, which adopts the following technical solution: A construction process for solidifying a soil road surface layer comprises the following steps: Prepare the base: level the roadbed, lay waste bricks, and roll and compact them to obtain the base; Prepare a high-strength solidified layer: lay high-strength solidified soil on the base layer and roll it to obtain a high-strength solidified soil layer with a thickness of 10-15 cm; prepare a protective layer: mix silicone emulsion, defoaming agent, hydrogenated silicone oil, silicon dioxide and water evenly to obtain a protective liquid, spray the protective liquid on the surface of the high-strength solidified soil layer, and then evenly sprinkle the wear-resistant agent on the protective liquid 2-3 times, dry it naturally and then grind it to form a protective layer with a thickness of 10-15 mm.
[0025] By adopting the above technical scheme, the base layer containing waste brick particles is compacted, high-strength solidified soil is laid, and finally protective liquid is sprayed, wear-resistant agent is sprinkled, and then it is dried and polished to obtain a road surface layer with high strength, good impermeability and wear resistance, and the construction method is simple.
[0026] In summary, this application has the following beneficial effects: 1. Since the present application uses yellow mud, pea gravel and fine sand as raw materials, and uses cement, sodium silicate and calcium carbonate as soil solidifiers, cement can produce hydration to form calcium hydroxide and CSH gel, and sodium silicate and calcium carbonate can react with cement to form calcium silicate gel, etc., which bond and solidify the soil and fill the gaps in the solidified body, so that the soil is consolidated and is not prone to volume shrinkage.
[0027] 2. In the present application, carbide slag, rice husk ash and epoxy resin are preferably used to pretreat the pea gravel, so that the porosity of the pea gravel is reduced, the density is increased, the strength is improved, and the surface hydrophobicity is enhanced, thereby enhancing the anti-seepage effect of the high-strength solidified soil.
[0028] 3. In this application, a base layer containing waste brick particles is used as the bottom, high-strength solidified soil is laid and then rolled to form a high-strength solidified soil layer, and then a protective liquid is sprayed and a wear-resistant agent is sprinkled to form a road surface layer with strong crack resistance, high compressive strength, anti-seepage effect and strong wear resistance. It is not easy to get dusty on sunny days and not easy to get slippery on rainy days. DETAILED DESCRIPTION
[0029] The following examples further illustrate the present application in detail.
[0030] Preparation Examples 1-4 of Wear Resistant Agents Preparation Example 1: (1) 50 g of clay, 15 g of fly ash and 30 g of water were mixed evenly, and 1 g of calcium lignin sulfonate was added. After mixing evenly, the mixture was added to a granulator, granulated, dried and ball-milled to obtain spherical bodies with a particle size of 100 μm. The clay was bentonite, the fly ash was Grade II fly ash, the fineness was 11.2%, the loss on ignition was 1.2%, the activity index was 76%, and the water requirement ratio was 100%; (2) the spherical body is mixed evenly with 1 g of polyvinyl alcohol, 65 g of polyimide and 400 g of water to form a mixed slurry, wherein the polyvinyl alcohol is PVA1788, and the polyimide is selected from Mitsui Chemicals of Japan, model PL450C; (3) The mixed slurry was spray granulated to obtain an anti-wear agent. The spray drying inlet temperature was 110° C., the outlet temperature was 130° C., the flow rate was 65 ml / min, and the atomization speed was 15000 rpm.
[0031] Preparation Example 2: (1) 20 g of clay, 5 g of fly ash and 15 g of water were mixed evenly, and 0.4 g of calcium lignin sulfonate was added. After mixing evenly, the mixture was added to a granulator, granulated, dried and ball-milled to obtain spherical bodies with a particle size of 150 μm. The clay was bentonite, the fly ash was grade II fly ash, the fineness was 11.2%, the loss on ignition was 1.2%, the activity index was 76%, and the water requirement ratio was 100%; (2) the spherical body is mixed evenly with 0.9 g polyvinyl alcohol, 25 g polyimide and 300 g water to form a mixed slurry, the polyvinyl alcohol is PVA1788, and the polyimide is selected from Mitsui Chemicals of Japan, model PL450C; (3) The mixed slurry was spray granulated to obtain an anti-wear agent. The spray drying inlet temperature was 115° C., the outlet temperature was 135° C., the flow rate was 60 ml / min, and the atomization speed was 15000 rpm.
[0032] Preparation Example 3: After 50g of clay, 15g of fly ash and 30g of water are mixed evenly, 1g of calcium lignin sulfonate is added, the mixture is mixed evenly, and the mixture is added to a granulator for granulation, drying and ball milling to obtain a wear-resistant agent with a particle size of 100μm. The clay is bentonite, the fly ash is grade II fly ash, the fineness is 11.2%, the loss on ignition is 1.2%, the activity index is 76%, and the water demand ratio is 100%.
[0033] Preparation Example 4: The difference from Preparation Example 1 is that calcium lignin sulfonate is not added. Example
[0034] Example 1: A high-strength solidified soil comprises the following raw materials by weight: 300 g of a curing agent, 600 g of fine sand, 300 g of yellow mud, 500 g of pea gravel and 250 g of water, wherein the curing agent comprises 240 g of Conch brand P.O42.5 silicate cement, 30 g of anhydrous sodium sulfate and 30 g of calcium carbonate with a particle size of 400 mesh, the fineness modulus of the fine sand is 2.3, and the particle size of the pea gravel is 2 cm.
[0035] Example 2: A high-strength solidified soil comprises the following raw materials by weight: 400g of a curing agent, 550g of fine sand, 350g of yellow mud, 350g of pea gravel and 30g of water, wherein the curing agent comprises 320g of Conch brand P.O42.5 silicate cement, 40g of anhydrous sodium sulfate and 40g of calcium carbonate with a particle size of 400 mesh, the fineness modulus of the fine sand is 2.3, and the particle size of the pea gravel is 1cm.
[0036] Example 3: A high-strength solidified soil comprises the following raw materials by weight: 300 g of a curing agent, 600 g of fine sand, 300 g of yellow mud, 500 g of pea gravel and 250 g of water, wherein the curing agent comprises 210 g of Conch brand P.O42.5 silicate cement, 45 g of anhydrous sodium sulfate and 45 g of calcium carbonate with a particle size of 400 mesh, the fineness modulus of the fine sand is 2.3, and the particle size of the pea gravel is 2 cm.
[0037] Example 4: A high-strength solidified soil, which is different from Example 1 in that the pea gravel is pretreated as follows: 200 g of carbide slag, 100 g of rice husk ash and water were mixed in a ratio of 2:1:1.5 to obtain a slurry, wherein the average particle size of the carbide slag was 5 μm, and the average particle size of the rice husk ash was 8 μm; 500 g of pea gravel was added to the slurry and stirred thoroughly, and then the pea gravel coated with the slurry was placed on a wire mesh and allowed to stand for 3 hours, and then cured in a constant temperature and humidity chamber at a temperature of 20° C. and a humidity of 95% for 28 days to obtain aggregate; 800g of epoxy resin and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane were mixed in a mass ratio of 10:1, aggregate was added, the mixture was fully stirred, and the mixture was spread out and allowed to stand for 24h. The epoxy resin emulsion was selected from Guangzhou Shanghe New Material Technology Co., Ltd., model number WEP-6858.
[0038] Example 5: A high-strength solidified soil, which is different from Example 1 in that the pea gravel is pretreated as follows: 180 g of carbide slag, 100 g of rice husk ash and water were mixed in a ratio of 1.8:1:1.4 to obtain a slurry, wherein the average particle size of the carbide slag was 5 μm, and the average particle size of the rice husk ash was 8 μm; 500 g of pea gravel was added to the slurry and stirred thoroughly, and then the pea gravel coated with the slurry was placed on a wire mesh and allowed to stand for 2 hours, and then cured in a constant temperature and humidity chamber at a temperature of 20° C. and a humidity of 95% for 28 days to obtain aggregate; 800g of epoxy resin and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane were mixed in a mass ratio of 10:0.8, aggregate was added, the mixture was fully stirred, and the mixture was spread out and allowed to stand for 20h. The epoxy resin emulsion was selected from Guangzhou Shanghe New Material Technology Co., Ltd., model number WEP-6858.
[0039] Example 6: A high-strength stabilized soil, which is different from Example 1 in that the pea gravel is pretreated as follows: 200 g of carbide slag, 100 g of rice husk ash and water were mixed in a ratio of 2:1:1.5 to obtain a slurry, wherein the average particle size of the carbide slag was 5 μm, and the average particle size of the rice husk ash was 8 μm; Add 500g of pea gravel into the slurry and stir thoroughly. Then place the pea gravel coated with slurry on a wire mesh and let it stand for 3h. Then, cure it in a constant temperature and humidity chamber at 20℃ and 95% for 28d.
[0040] Example 7: A high-strength stabilized soil, which is different from Example 1 in that the pea gravel is pretreated as follows: 800 g of epoxy resin and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane were mixed in a mass ratio of 10:1, 500 g of pea gravel was added, the mixture was fully stirred, and the mixture was spread out and allowed to stand for 24 h. The epoxy resin emulsion was selected from Guangzhou Shanghe New Material Technology Co., Ltd., model number WEP-6858.
[0041] Example 8: A high-strength solidified soil comprises the following raw materials by weight: 1000g of a solidifying agent, 3500g of yellow mud, and 500g of water. The solidifying agent comprises 800g of cement, 100g of sodium silicate, and 100g of calcium carbonate. The particle size of the calcium carbonate is 400 mesh. The cement is Conch brand PO 42.5 silicate cement.
[0042] Example 9: A high-strength solidified soil, comprising the following raw materials by weight: 950g of curing agent, 3450g of yellow mud, and 450g of water. The curing agent comprises 760g of cement, 95g of sodium silicate and 95g of calcium carbonate. The particle size of calcium carbonate is 400 mesh. The cement is Conch brand P.O42.5 silicate cement.
[0043] Example 10: A high-strength solidified soil, comprising the following raw materials in parts by weight: 1000g of a solidifying agent, 3500g of yellow mud, and 500g of water. The solidifying agent comprises 700g of cement, 150g of sodium silicate, and 150g of calcium carbonate. The particle size of the calcium carbonate is 400 mesh. The cement is Conch brand P.O42.5 silicate cement.
[0044] Comparative Example Comparative Example 1: A high-strength solidified soil, which differs from Example 1 in that an equal amount of slaked lime is used to replace the solidifying agent.
[0045] Comparative Example 2: A high-strength solidified soil, which differs from Example 1 in that an equal amount of cement is used to replace the solidifying agent.
[0046] Comparative Example 3: A high-strength solidified soil, which differs from Example 8 in that an equal amount of slaked lime is used to replace the solidifying agent.
[0047] Comparative Example 4: A high-strength solidified soil, which differs from Example 8 in that an equal amount of cement is used to replace the solidifying agent.
[0048] Application Example I Application Example I-1: A solidified soil road surface layer, comprising a base layer, a high-strength solidified soil layer and a protective layer in contact with each other in sequence, wherein the construction process of the solidified soil road surface layer comprises the following steps: S1. Preparation of base layer: Level the roadbed, lay waste brick particles, roll and compact them to obtain the base layer. The waste brick particles include 5mm and 15mm in a mass ratio of 1:2, and the base layer thickness is 25cm; S2. Preparing a high-strength solidified soil layer: According to the raw material dosage in Example 1, the raw materials are mixed to obtain a high-strength solidified soil, which is laid on the base layer and rolled to obtain a high-strength solidified layer with a thickness of 15 cm; S3. Prepare a protective layer: evenly mix 8 kg of silicone emulsion, 0.02 kg of defoaming agent, 0.04 kg of hydrogenated silicone oil, 0.5 kg of silicon dioxide and 2 kg of water to prepare a protective liquid, spray the protective liquid on the surface of the high-strength cured layer, and then evenly sprinkle 0.5 kg of the wear-resistant agent prepared in Preparation Example 1 on the protective liquid twice, dry it naturally and then polish it to form a protective layer with a thickness of 15 mm.
[0049] Application Example I-2: A solidified soil road surface layer, comprising a base layer, a high-strength solidified soil layer and a protective layer in contact with each other in sequence, wherein the construction process of the solidified soil road surface layer comprises the following steps: S1. Preparation of base layer: Level the roadbed, lay waste brick particles, roll and compact them to obtain the base layer. The waste brick particles include 5mm and 15mm in a mass ratio of 1:2, and the base layer thickness is 20cm; S2. Preparing a high-strength solidified soil layer: According to the raw material dosage in Example 2, the raw materials are mixed to obtain a high-strength solidified soil, which is laid on the base layer and rolled to obtain a high-strength solidified layer with a thickness of 10 cm; S3. Prepare a protective layer: evenly mix 4 kg of silicone emulsion, 0.01 kg of defoaming agent, 0.02 kg of hydrogenated silicone oil, 0.1 kg of silicon dioxide and 1 kg of water to prepare a protective liquid, spray the protective liquid on the surface of the high-strength cured layer, and then evenly sprinkle 0.3 kg of the wear-resistant agent prepared in Preparation Example 2 on the protective liquid in 3 times, dry it naturally and then polish it to form a protective layer with a thickness of 10 mm.
[0050] Application Example I-3: A solidified earth road surface layer, which differs from Application Example I-1 in that, in step S3, the wear-resistant agent is prepared by Preparation Example 3.
[0051] Application Example I-4: A solidified earth road surface layer, which differs from Application Example I-1 in that, in step S3, the wear-resistant agent is prepared by Preparation Example 4.
[0052] Application Example I-5: A cured earth road surface layer, which differs from Application Example I-1 in that no wear-resistant agent is added to the protective layer.
[0053] Application Example I-6: A solidified soil road surface layer, which differs from Application Example I-1 in that no protective layer is provided.
[0054] Application Example I-7: A solidified soil road surface layer, which differs from Application Example I-1 in that the high-strength solidified soil in step S2 adopts the amount in Example 8.
[0055] Performance testing 1. Performance test of high-strength curing agent: prepare high-strength cured soil according to the methods in Examples 1-10 and Comparative Examples 1-4, test the compressive strength according to the method in GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", and test the permeability coefficient according to GB / T50123-2019 "Standard for Geotechnical Test Methods", and record the test results in Table 1.
[0056] Table 1 Performance test of high strength solidified soil The high-strength solidified soil prepared in Examples 1-3 has high compressive strength, which is higher than that when slaked lime and cement are used as solidifying agents, and has a tighter structure and better impermeability.
[0057] In Example 4 and Example 5, rice husk ash, carbide slag, etc. are used to pretreat the pea gravel. It can be seen that the high-strength solidified soil prepared in Example 4 and Example 5 has better performance.
[0058] In Example 6, carbide slag and rice husk ash were used to make a slurry to wrap the pea gravel, and in Example 7, epoxy resin emulsion was used to wrap the pea gravel. Compared with Example 4, the impermeability of the solidified soil in Example 6 decreased, and the strength of the solidified soil in Example 7 decreased.
[0059] In Examples 8-10, a curing agent, yellow mud and water were used to prepare the cured soil, and it can be seen that the cured soil also has a strong compressive strength.
[0060] 2. Performance measurement of the cured soil road surface layer: Prepare the cured soil road surface layer according to the method in Application Example I1-7, and test it according to the following method, and record the test results in Table 2.
[0061] 1. Wear amount: Prepare a cubic specimen with a specification of 150mm×150mm. During the test, the initial mass m1 of the specimen is the mass of the specimen after 30r of wear, and the mass m2 of the specimen after wear is the remaining mass of the specimen after 60r of wear. The wear amount per unit area of the specimen is calculated according to the following formula: G=(m1-m2) / V, G is the wear amount per unit area (kg / m 2 ); V is the area of the worn surface (m 2 ).
[0062] 2. Seepage height: Test in accordance with GB / T50082-2009 "Test methods for long-term performance and durability of ordinary concrete".
[0063] 3. Flexural strength: The compressive strength is tested according to the method in GB / T17671-2021 "Standard Test Methods for Physical and Mechanical Properties of Concrete".
[0064] Table 2 Performance test of solidified soil road surface Table 2 shows that Application Example I1 and Application Example I-2 use the high-strength solidified soil prepared by the formula in Example 1 and Example 2 to form a high-strength solidified soil layer, and provide a protective layer containing the wear-resistant agent prepared by Preparation Example 1 and Preparation Example 2, respectively, which can effectively improve the wear resistance, crack resistance and permeability resistance of the solidified soil road surface layer.
[0065] The wear-resistant agent in the protective layer in Application Example I-3 is made from Preparation Example 3, wherein polyimide or the like is not used for spray drying. Compared with Application Example I-1, the wear resistance of the cured earth road surface layer prepared therefrom decreases, the anti-seepage ability weakens, and the anti-flexural effect deteriorates.
[0066] In Application Example I-4, the wear-resistant agent prepared in Preparation Example 4 was used. Compared with Preparation Example 1, calcium lignin sulfonate was not added. Comparison of the data in Table 2 shows that the wear-resistant effect of the road surface layer prepared in Application Example I-4 is weakened.
[0067] No anti-wear agent was added in Application Example I-5, and no protective layer was set in Application Example I-6. The data in Table 2 showed that compared with Application Example I-1, the wear amount of the road surface layers made in Application Example I-5 and Application Example I-6 increased, and the anti-seepage effect and crack resistance were weakened.
[0068] In Application Example I-7, the amount of solidified soil used in Example 8 was adopted, and it can be seen that the impermeability and wear resistance did not deteriorate much, and the flexural strength decreased slightly.
[0069] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high-strength solidified soil, characterized in that: The invention comprises the following raw materials in parts by weight: 300-1000 parts of a curing agent, 0-600 parts of fine sand, 300-3500 parts of yellow mud, 0-500 parts of pea gravel and 250-500 parts of water. The curing agent comprises cement, sodium silicate and calcium carbonate in a mass ratio of 7-8:1-1.5:1-1.
5.
2. The high-strength stabilized soil according to claim 1, characterized in that: The high-strength solidified soil comprises the following raw materials in parts by weight: 950-1000 parts of a curing agent, 3450-3500 parts of yellow mud, and 450-500 parts of water. The curing agent comprises cement, sodium silicate and calcium carbonate in a mass ratio of 8:1:
1.
3. The high-strength stabilized soil according to claim 1, characterized in that: The high-strength solidified soil comprises the following raw materials in parts by weight: 300-400 parts of a curing agent, 550-600 parts of fine sand, 300-350 parts of yellow mud, 350-500 parts of pea gravel, and 250-300 parts of water. The curing agent comprises cement, sodium silicate, and calcium carbonate in a mass ratio of 8:1:
1.
4. The high-strength stabilized soil according to claim 3, characterized in that: The particle size of the pea gravel is 1-2 cm.
5. The high-strength stabilized soil according to claim 4, characterized in that: The pea gravel is pretreated as follows: carbide slag, rice husk ash and water are mixed in a ratio of 1.8-2:1:1.4-1.5 to obtain a slurry; Add pea gravel to the slurry, stir thoroughly, then place the pea gravel coated with slurry on a wire mesh and let it stand for 2-3 hours, then maintain constant temperature and humidity for 28 days to obtain aggregate; Mix epoxy resin and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane in a mass ratio of 10:0.8-1, add aggregate, stir thoroughly, spread evenly and let stand for 20-24 hours.
6. A solidified soil road surface layer, characterized in that: The invention comprises a base layer containing waste brick particles and a high-strength solidified soil layer located above the base layer, wherein the high-strength solidified soil layer is formed by laying and rolling the high-strength solidified soil described in any one of claims 1 to 5 on the base layer.
7. The solidified soil road surface layer according to claim 6, characterized in that: The solidified soil road surface layer also includes a protective layer located above the high-strength solidified soil layer, and the protective layer includes 4-8 parts by weight of silicone emulsion and 0.3-0.5 parts by weight of wear resistance agent, 0.01-0.02 parts by weight of defoaming agent, 0.02-0.04 parts by weight of hydrogenated silicone oil, 0.1-0.5 parts by weight of silicon dioxide, and 1-2 parts by weight of water.
8. The solidified soil road surface layer according to claim 7, characterized in that: The preparation method of the wear-resistant agent comprises the following steps: In parts by weight, 2-5 parts of clay, 0.5-1.5 parts of fly ash and 1.5-3 parts of water are mixed, and 0.04-0.1 parts of calcium lignin sulfonate are added, and the mixture is granulated, dried, and ball-milled to obtain spherical bodies with a particle size of 100-150 μm; The spherical body is mixed with 0.09-0.1 parts of polyvinyl alcohol, 2.5-6.5 parts of polyimide and 30-40 parts of water to form a mixed slurry; The mixed slurry is spray granulated, dried and sintered to obtain the wear-resistant agent. The spray drying inlet temperature is 110-115°C, the outlet temperature is 130-135°C, and the flow rate is 60-65ml / min.
9. The solidified soil road surface layer according to claim 6, characterized in that: The thickness of the high-strength solidified soil layer is 10-15 cm, and the thickness of the protective layer is 10-15 mm.
10. The construction process of the solidified soil road surface layer according to any one of claims 6 to 9, characterized in that: The following steps are involved: Prepare the base: level the roadbed, lay waste bricks, and roll and compact them to obtain the base; Preparing a high-strength solidified layer: laying high-strength solidified soil on the base layer and rolling it to obtain a high-strength solidified soil layer; Prepare the protective layer: mix the organosilicon emulsion, defoaming agent, hydrogenated silicone oil, silicon dioxide and water evenly to prepare the protective liquid, spray the protective liquid on the surface of the high-strength solidified soil layer, sprinkle the wear-resistant agent evenly on the protective liquid 2-3 times, dry it naturally and then polish it to form a protective layer.
Citation Information
Patent Citations
Solidified soil and anti-fouling and anti-seepage treatment method for large coal yards
CN108191310A
An epoxy resin grouting material and its preparation method
CN114933782A
Soil paving material and method for paving using thereof
KR100775360B1
Soil coagulant and paving method using thiis
KR100922196B1
Environmentally friendly ground foundation materials, structure of pavement layer using ground foundation materials and construction method for pavement of farm road and street
KR1020050016864A