Manganese zinc ferrite material as well as preparation method and application thereof

By adjusting the composition and preparation process of manganese-zeb ferrite materials, the existing materials have been solved inadequate performance under extreme conditions, and the characteristics of high frequency, high magnetic permeability and high Curie temperature are achieved, which meets the automotive electronics and other fields wide temperature wide frequency requirements.

CN118908707AInactive Publication Date: 2024-11-08HENGDIAN GRP DMEGC MAGNETICS CO LTD +1

Patent Information

Application Number
CN202410964233.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing manganese-zeb ferrite materials have insufficient performance under extreme temperature and frequency conditions, and cannot meet the wide temperature, wide frequency and high permeability requirements in automotive electronics and other fields.

Method used

By adjusting the mole percentage of Fe2O3, ZnO and MnO, and introducing CaO, Bi2O3 and MoO as auxiliary components, combined with a specific preparation process, manganese-zeb iron with high frequency, high magnetic permeability, high Curie temperature and low temperature coefficient were prepared. Oxygen material.

Benefits of technology

The manganese-zeb ferrite material has been achieved in a stable operation within the temperature range of 0-120℃, with the magnetic permeability maintained at 10000-11000, the Curie temperature is greater than 150℃, and the magnetic permeability of 300KHz does not drop, meeting the application needs in extreme environments .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004951271910000141
    Figure BDA0004951271910000141
  • Figure BDA0004951271910000142
    Figure BDA0004951271910000142
  • Figure BDA0004951271910000151
    Figure BDA0004951271910000151
Patent Text Reader

Abstract

The invention provides a manganese zinc ferrite material and a preparation method and application thereof, the manganese zinc ferrite material comprises a main component, an additive and an auxiliary component, the main component comprises 50.5-52.5 mol% of Fe2O3, 17.0-19.5 mol% of ZnO, and the balance MnO; the additive comprises CaO; and the auxiliary components comprise Bi2O3 and MoO, or comprise CoO, Bi2O3 and MoO. According to the manganese zinc ferrite material disclosed by the invention, through component matching, the manganese zinc ferrite material has the characteristics of high frequency, high magnetic conductivity, high Curie temperature and low temperature coefficient, and stable work of the manganese zinc ferrite material in a temperature range of 0-120 DEG C in the electronic field is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a manganese-zinc ferrite material and a preparation method and application thereof. Background Art

[0002] At present, high permeability manganese-zinc ferrite is widely used in the fields of electronic signal transmission, anti-electromagnetic interference technology, environmental protection and energy saving, and automotive electronics market. In particular, when manganese-zinc ferrite is used in electronic products and devices, its comprehensive performance often needs to be improved. For example, automotive electronics requires wide temperature, wide frequency and high permeability manganese-zinc soft magnetic ferrite. In hot areas, if a car needs to be stopped during full load use, the heat from the exhaust pipe of the car will make the engine room reach more than 100°C. In cold areas, the outdoor temperature is as low as -40°C. In extreme weather, the normal operation of automotive ferrites requires low permeability changes within the temperature range, that is, excellent temperature characteristics.

[0003] Therefore, it is necessary to match the formula and process to develop materials with high magnetic permeability, high Curie temperature, wide frequency and wide temperature. The manganese-zinc ferrite with a very small temperature coefficient of -40 to 125°C disclosed in the prior art has 50.5 to 52.5 mol% of iron oxide, 29 to 30 mol% of manganese oxide, and the rest is zinc oxide, and the magnetic permeability is only about 5000, which cannot meet the performance requirements for use under extreme conditions.

[0004] For example, CN 106747396A discloses a ferrite material, whose valley point between the second peak and the first peak of magnetic permeability at 25°C to 80°C is greater than 8000, and the Curie temperature is greater than 150°C. Its main components are iron oxide in the range of 52.0-53.0 mol%, zinc oxide in the range of 17.0-20.5 mol%, and the rest is manganese oxide. The auxiliary agents are analytically pure CuO, CaCO3, Ta2O5, In2O3, and Bi2O3, which still cannot meet the requirements for use under extreme conditions. For another example, in the manganese-zinc ferrite disclosed in CN 101050108A, manganese oxide is in the range of 21.5-26.5 mol%, zinc oxide is in the range of 20.5-25.5 mol%, and the rest is iron oxide. However, the magnetic permeability does not drop at 100 KHz, and the high Curie temperature is not mentioned.

[0005] Based on the above research, there is a need to provide a manganese-zinc ferrite material, which has the characteristics of high magnetic permeability, high Curie temperature, wide bandwidth and low temperature coefficient and can be used in extreme environments. Summary of the invention

[0006] The object of the present invention is to provide a manganese-zinc ferrite material and a preparation method and application thereof. The manganese-zinc ferrite material has high frequency, high magnetic permeability, high Curie temperature and low temperature coefficient characteristics through component matching, so that the manganese-zinc ferrite material can work stably in the temperature range of 0-120°C in the electronic field.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a manganese-zinc ferrite material, the manganese-zinc ferrite material comprising a main component, an additive and an auxiliary component, the main component comprising 50.5-52.5 mol% of Fe2O3, 17.0-19.5 mol% of ZnO, and the remainder being MnO;

[0009] The additive includes CaO;

[0010] The auxiliary components include Bi2O3 and MoO, or include CoO, Bi2O3 and MoO.

[0011] The present invention adopts Fe2O3, ZnO and MnO with a specific molar percentage as main components, adopts Bi2O3 and MoO, or CoO, Bi2O3 and MoO as auxiliary components, and adopts CaO as an additive. Through the coordination of all components, a manganese-zinc ferrite material with high frequency, high magnetic permeability, high Curie temperature and low temperature coefficient characteristics is obtained; wherein, for CaO, the resistivity of the product can be improved, and at the same time, with the anisotropy constant K1 of CoO>0, CoO 2+ The K1 value contributed by the ions decreases sharply with increasing temperature, so for the temperature range where the offset point of K1 = 0 is lower than the Curie temperature, and the cobalt oxide is combined with Fe 2+ Ions can adjust the situation where K1 is 0.

[0012] The 50.5-52.5 mol% Fe2O3 may be, for example, 50.5 mol%, 51 mol%, 51.5 mol%, 52 mol% or 52.5 mol%, and the 17.0-19.5 mol% ZnO may be, for example, 17 mol%, 17.5 mol%, 18 mol%, 18.5 mol%, 19 mol% or 19.5 mol%, but are not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0013] Preferably, the CaO is coated on the surface of the main component.

[0014] Preferably, the main component includes 50.5-52.5 mol% Fe2O3, for example, 50.5 mol%, 51 mol%, 51.5 mol%, 52 mol% or 52.5 mol%, 17.0-19.5 mol% ZnO, for example, 17 mol%, 17.5 mol%, 18 mol%, 18.5 mol%, 19 mol% or 19.5 mol%, and 30-30.5 mol% MnO, for example, 30 mol%, 30.1 mol%, 30.2 mol%, 30.3 mol%, 30.4 mol% or 30.5 mol%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] Preferably, based on the total weight of the main components as 100%, the CaO content is 400-2000ppm, for example, it can be 400ppm, 600ppm, 800ppm, 1000ppm, 1200ppm, 1400ppm, 1600ppm, 1800ppm or 2000ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, based on the total weight of the main component as 100%, the auxiliary components include 0-2000ppm CoO, for example, 0ppm, 500ppm, 1000ppm, 1500ppm or 2000ppm, 200-2000ppm Bi2O3, for example, 200ppm, 500ppm, 1000ppm, 1500ppm or 2000ppm, and 200-2000ppm MoO, for example, 200ppm, 500ppm, 1000ppm, 1500ppm or 2000ppm, but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, based on the total weight of the main component as 100%, the auxiliary component also includes 200-2000ppm CaCO3, for example, it can be 200ppm, 500ppm, 1000ppm, 1500ppm or 2000ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the manganese-zinc ferrite material has a magnetic permeability μ i In the range of 10000-11000, for example, it can be 10000, 10200, 10400, 10600, 10800 or 11000, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the Curie temperature of the manganese-zinc ferrite material is ≥150°C, for example, it can be 150°C, 151°C, 152°C, 153°C, 154°C or 155°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the manganese-zinc ferrite material has a magnetic permeability μ at 300 KHz. i ≥9500, for example, it can be 9500, 9600, 9700, 9800 or 9900, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] The manganese-zinc ferrite material of the present invention has a high initial magnetic permeability and a low temperature coefficient in the temperature range of 0 to 120° C., a 300KHz magnetic permeability μi≥9500, and a Curie temperature greater than 150° C.

[0022] In a second aspect, the present invention provides a method for preparing the manganese-zinc ferrite material as described in the first aspect, the preparation method comprising the following steps:

[0023] (1) mixing and pre-calcining the main component and the additive to obtain a pre-calcined material;

[0024] (2) mixing the auxiliary components with the pre-burned material in step (1) to obtain a mixed material;

[0025] (3) tempering the mixed material in step (2) to obtain a tempered material;

[0026] (4) mixing the binder with the tempered material in step (3) and granulating the mixture to obtain a granular material;

[0027] (5) Pressing the granular material in step (4) into a shape, and then sintering it to obtain the manganese-zinc ferrite material.

[0028] The present invention adopts the method of adding nano-scale CaO into the main component by ball milling once, so as to better coat it and thus improve the resistivity, and cooperate with the sintering process to improve the frequency characteristics. If CaO is added together with the auxiliary components instead of coating the main component, the coating effect on the main component is not good, which may lead to low resistance of the powder after the sintering process, and fail to achieve a good effect of improving the frequency characteristics.

[0029] Preferably, the pre-burning temperature in step (1) is 700-800°C, for example, 700°C, 750°C or 800°C, and the time is 2-3h, for example, 2h, 2.5h or 3h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the mixing method in step (1) comprises ball milling.

[0031] Preferably, the mixing method in step (2) includes sand milling and / or ball milling.

[0032] Preferably, the tempering temperature in step (3) is 700-850°C, for example, 700°C, 750°C, 800°C or 850°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the amount of the binder added in step (4) is 5-10wt% of the tempering material in step (3), for example, it can be 5wt%, 7wt%, 9wt% or 9wt%, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 7-9wt%.

[0034] Preferably, the sintering in step (5) is carried out in a protective gas, wherein the oxygen content in the protective gas is 3-21 vol%, for example, 3 vol%, 5 vol%, 10 vol%, 15 vol%, 20 vol% or 21 vol%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] Preferably, the sintering in step (5) is first carried out in a protective gas with an oxygen content of 19-21 vol%, for example, 19 vol%, 20 vol% or 21 vol%, at a temperature of 600-700°C, for example, 600°C, 650°C or 700°C, for 1-5 h, for example, 1 h, 3 h or 5 h, then the temperature is increased to 1000-1100°C, for example, 1000°C, 1050°C or 1100°C, for 4-8 h, for example, 4 h, 6 h or 8 h, and finally in a protective gas with an oxygen content of 3-7 vol%, for example, 3 vol%, 5 vol% or 7 vol%, at a temperature of 1250-1360°C, for example, 1250°C, 1300°C or 1360°C, for 5-7 h, for example, 5 h, 6 h or 7 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0036] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:

[0037] (1) After the main component and CaO are ball-milled and dried, they are pre-fired at 700-800° C. for 2-3 hours in an air atmosphere to obtain a pre-fired material;

[0038] (2) sand-milling and ball-milling the auxiliary components and the pre-burned material in step (1), and drying to obtain a mixed material;

[0039] (3) tempering the mixed material in step (2) at 700-850° C. to obtain a tempered material;

[0040] (4) mixing the tempered material of step (3) with 7-9 wt % of a binder and granulating the mixture to obtain a granular material;

[0041] (5) Pressing the granular material prepared in step (4) into a mold, firstly keeping the temperature at 600-700° C. in a protective gas with an oxygen content of 19-21 vol%, then heating the temperature to 1000-1100° C. and keeping the temperature for 4-8 h, and finally keeping the temperature at 1250-1360° C. in a protective gas with an oxygen content of 3-7 vol% for 5-7 h, to obtain the manganese-zinc ferrite material.

[0042] In a third aspect, the present invention provides an application of the manganese-zinc ferrite material as described in the first aspect, wherein the application includes use in the field of automotive electronics.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] The present invention adopts Fe2O3, ZnO and MnO with specific molar percentage as main components, CoO, Bi2O3 and MoO as auxiliary components, and CaO as an additive. By matching all components and a specific preparation method, a manganese-zinc ferrite material with high frequency, high magnetic permeability, high Curie temperature and low temperature coefficient characteristics is obtained. The manganese-zinc ferrite material has a magnetic permeability of 10000-11000 in the temperature range of 0-120°C, a lower temperature coefficient in the range, a higher Curie temperature, a Curie temperature greater than 150°C, and a magnetic permeability that does not drop at 300KHz and is greater than or equal to 9500. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0046] Example 1

[0047] This embodiment provides a manganese-zinc ferrite material, the manganese-zinc ferrite material includes a main component, an additive and an auxiliary component, the main component includes 52.0 mol% Fe2O3, 17.81 mol% ZnO, and 30.2 mol% MnO;

[0048] Based on the total weight of the main component being 100%, the additive is 500 ppm of CaO; based on the total weight of the main component being 100%, the auxiliary component includes 1500 ppm of CoO, 400 ppm of Bi2O3 and 200 ppm of MoO;

[0049] The preparation method of the manganese-zinc ferrite material comprises the following steps:

[0050] (1) The main component and nano-CaO are placed in a ball mill according to the formula amount to be mixed until uniform, placed in an oven for drying, and then pre-calcined at 750° C. for 2.5 hours in an air atmosphere to obtain a pre-calcined material;

[0051] (2) wet-grinding the auxiliary components and the pre-burnt material in step (1) for 65 minutes, ball-milling for 30 minutes, and drying to obtain a mixed material;

[0052] (3) tempering the mixed material in step (2) at 760° C. to obtain a tempered material;

[0053] (4) mixing the tempered material of step (3) with 8 wt % of PVA (polyvinyl alcohol) to form granules, and sieving to obtain granular material;

[0054] (5) The granular material described in step (4) is pressed into a blank with a size of H25×15×8 by a press, and then sintered at 600°C for 3.5 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, and then sintered at 1100°C for 6 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, and finally kept at 1320°C for 6 hours in a nitrogen atmosphere with an oxygen content of 4 vol%, and cooled under a balanced oxygen partial pressure to obtain a powder core for testing.

[0055] Example 2

[0056] This embodiment provides a manganese-zinc ferrite material, the manganese-zinc ferrite material includes a main component, an additive and an auxiliary component, the main component includes 51.15 mol% Fe2O3, 18.6 mol% ZnO, and 30.25 mol% MnO;

[0057] Based on the total weight of the main component being 100%, the additive is 400 ppm of CaO; based on the total weight of the main component being 100%, the auxiliary component includes 2000 ppm of CoO, 450 ppm of Bi2O3 and 200 ppm of MoO;

[0058] The preparation method of the manganese-zinc ferrite material comprises the following steps:

[0059] (1) The main component and nano-CaO are placed in a ball mill according to the formula amount to be mixed until uniform, placed in an oven for drying, and then pre-calcined at 730° C. for 3 h in an air atmosphere to obtain a pre-calcined material;

[0060] (2) wet-grinding the auxiliary components and the pre-burnt material in step (1) for 70 minutes, ball-milling for 30 minutes, and drying to obtain a mixed material;

[0061] (3) tempering the mixed material in step (2) at 760° C. to obtain a tempered material;

[0062] (4) mixing the tempered material of step (3) with 10 wt% of PVA to form granules, and sieving to obtain granules;

[0063] (5) The granular material described in step (4) is pressed into a blank with a size of H25×15×8 by a press, and then sintered at 650°C for 4.5 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, and then sintered at 1080°C for 6 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, and finally kept at 1350°C for 5 hours in a nitrogen atmosphere with an oxygen content of 7 vol%, and cooled under equilibrium oxygen partial pressure to obtain a powder core for testing.

[0064] Example 3

[0065] This embodiment provides a manganese-zinc ferrite material, the manganese-zinc ferrite material includes a main component, an additive and an auxiliary component, the main component includes 52.23 mol% Fe2O3, 17.63 mol% ZnO, and 30.14 mol% MnO;

[0066] Based on the total weight of the main component being 100%, the additive is 600 ppm of CaO; based on the total weight of the main component being 100%, the auxiliary component includes 2000 ppm of CoO, 450 ppm of Bi2O3 and 200 ppm of MoO;

[0067] The preparation method of the manganese-zinc ferrite material comprises the following steps:

[0068] (1) The main component and nano-CaO are placed in a ball mill according to the formula amount to be mixed until uniform, placed in an oven for drying, and then pre-calcined at 800° C. for 2 h in an air atmosphere to obtain a pre-calcined material;

[0069] (2) wet-grinding the auxiliary components and the pre-burnt material in step (1) for 60 minutes, ball-milling for 30 minutes, and drying to obtain a mixed material;

[0070] (3) tempering the mixed material in step (2) at 780° C. to obtain a tempered material;

[0071] (4) mixing the tempered material in step (3) with 6 wt % PVA to form granules, and sieving to obtain granules;

[0072] (5) The granular material described in step (4) is pressed into a blank with a size of H25×15×8 by a press, and then sintered at 700°C for 1.5 h in a nitrogen atmosphere with an oxygen content of 21 vol%, and then sintered at 1100°C for 6 h in a nitrogen atmosphere with an oxygen content of 21 vol%, and finally kept at 1320°C for 5 h in a nitrogen atmosphere with an oxygen content of 4 vol%, and cooled under a balanced oxygen partial pressure to obtain a powder core for testing.

[0073] Example 4

[0074] This embodiment provides a manganese-zinc ferrite material, which includes a main component, an additive and an auxiliary component, wherein the main component includes 52.34 mol% of Fe2O3, 17.6 mol% of ZnO, and 30-30.06 mol% of MnO;

[0075] Based on the total weight of the main component being 100%, the additive is 600 ppm of CaO; based on the total weight of the main component being 100%, the auxiliary component includes 3000 ppm of CoO, 500 ppm of Bi2O3 and 200 ppm of MoO;

[0076] The preparation method of the manganese-zinc ferrite material comprises the following steps:

[0077] (1) The main component and nano-CaO are placed in a ball mill according to the formula amount to be mixed until uniform, placed in an oven for drying, and then pre-calcined at 750° C. for 3 hours in an air atmosphere to obtain a pre-calcined material;

[0078] (2) wet-grinding the auxiliary components and the pre-burnt material in step (1) for 70 minutes, ball-milling for 30 minutes, and drying to obtain a mixed material;

[0079] (3) tempering the mixed material in step (2) at 700° C. to obtain a tempered material;

[0080] (4) mixing the tempered material of step (3) with 5 wt% of PVA to form granules, and sieving to obtain granules;

[0081] (5) The granular material described in step (4) is pressed into a blank with a size of H25×15×8 by a press, and then sintered at 700°C for 2 h in a nitrogen atmosphere with an oxygen content of 21 vol%, and then sintered at 1100°C for 6 h in a nitrogen atmosphere with an oxygen content of 21 vol%, and finally kept at 1360°C for 5 h in a nitrogen atmosphere with an oxygen content of 7 vol%, and cooled under a balanced oxygen partial pressure to obtain a powder core for testing.

[0082] Example 5

[0083] This embodiment provides a manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the auxiliary component further includes 1000 ppm of CaCO3.

[0084] Example 6

[0085] This embodiment provides a manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the auxiliary component does not include CoO and the content thereof is 0 ppm, that is, does not include CoO.

[0086] Example 7

[0087] This embodiment provides a manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the nano-scale CaO in step (1) of the preparation method is mixed with the pre-sintered material together with the auxiliary components in step (2).

[0088] Example 8

[0089] The present embodiment provides a manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that in step (5) of its preparation method, the material is first sintered at a temperature of 1100°C for 6 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, and finally kept warm at a temperature of 1320°C for 6 hours in a nitrogen atmosphere with an oxygen content of 4 vol%.

[0090] Comparative Example 1

[0091] This comparative example provides a manganese-zinc ferrite material, which includes a main component and an auxiliary component, wherein the main component includes 52.74 mol% of Fe2O3, 20.29 mol% of ZnO, and 26.97 mol% of MnO;

[0092] Based on the total weight of the main component being 100%, the auxiliary component includes 0.02wt% of CaCO3, 0.02wt% of Ta2O5, 0.02wt% of In2O3 and 0.01wt% of Bi2O3;

[0093] The preparation method of the manganese-zinc ferrite material comprises the following steps:

[0094] (1) The main components are placed in a ball mill according to the formula amount to be mixed until uniform, placed in an oven for drying, and then pre-calcined at 880° C. for 2.5 hours in an air atmosphere to obtain a pre-calcined material;

[0095] (2) wet-grinding the auxiliary components and the pre-sintered material in step (1) for 65 minutes and ball-milling for 30 minutes, and then sieving the ferrite granules obtained by spray granulation;

[0096] (3) The sieved material obtained by sieving in step (2) is pressed into a blank with a size of H25×15×8 by a press, and then sintered at a temperature of 1330°C for 6 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, and finally kept at a temperature of 1370°C for 1.5 hours in a nitrogen atmosphere with an oxygen content of 4 vol%, and cooled under a balanced oxygen partial pressure to obtain a powder core for testing.

[0097] Comparative Example 2

[0098] This comparative example provides a manganese-zinc ferrite material, which includes a main component and an auxiliary component, wherein the main component includes 52.5 mol% of Fe2O3, 23 mol% of ZnO, and 24.5 mol% of MnO;

[0099] Based on the total weight of the main component being 100%, the auxiliary component includes 100 ppm of CaCO3, 200 ppm of Bi2O3, 100 ppm of V2O5 and 200 ppm of MoO;

[0100] The preparation method of the manganese-zinc ferrite material comprises the following steps:

[0101] (1) The main components are placed in a ball mill according to the formula amount to be mixed until uniform, placed in an oven for drying, and then pre-calcined at 900° C. for 3 h in an air atmosphere to obtain a pre-calcined material;

[0102] (2) wet-grinding the auxiliary components and the pre-sintered material in step (1) for 65 minutes and ball-milling for 30 minutes, and then sieving the ferrite granules obtained by spray granulation;

[0103] (3) The sieved material obtained by sieving in step (2) is pressed into a blank with a size of H25×15×8 by a press, and then sintered at 1300°C for 6 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, and finally kept at 1390°C for 1.5 hours in a nitrogen atmosphere with an oxygen content of 4 vol%, and cooled under a balanced oxygen partial pressure to obtain a powder core for testing.

[0104] Comparative Example 3

[0105] This comparative example provides a manganese-zinc ferrite material, which includes a main component and an auxiliary component, wherein the main component includes 52.8 mol% of Fe2O3, 25.7 mol% of ZnO, and 21.5 mol% of MnO;

[0106] Based on the total weight of the main component being 100%, the auxiliary component includes 400 ppm of CaCO3, 400 ppm of Bi2O3 and 200 ppm of MoO;

[0107] The preparation method of the manganese-zinc ferrite material comprises the following steps:

[0108] (1) The main components are placed in a ball mill according to the formula amount to be mixed until uniform, placed in an oven for drying, and then pre-calcined at 890° C. for 2.5 hours in an air atmosphere to obtain a pre-calcined material;

[0109] (2) wet-grinding the auxiliary components and the pre-sintered material in step (1) for 65 minutes and ball-milling for 30 minutes, and then sieving the ferrite granules obtained by spray granulation;

[0110] (3) The sieved material obtained by sieving in step (2) is pressed into a blank with a size of H25×15×8 by a press, and then sintered at a temperature of 1310°C for 6 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, and finally kept at a temperature of 1370°C for 3 hours in a nitrogen atmosphere with an oxygen content of 4 vol%, and cooled under a balanced oxygen partial pressure to obtain a powder core for testing.

[0111] Comparative Example 4

[0112] This comparative example provides a manganese-zinc ferrite material, which is the same as Example 1 except that it does not include CaO;

[0113] The preparation method of the manganese-zinc ferrite material is the same as that of Example 1 except that CaO is not added.

[0114] The performance indicators of the manganese-zinc ferrite materials described in the above embodiments and comparative examples under different conditions are shown in Tables 1-3:

[0115] Table 1

[0116]

[0117] Table 2

[0118]

[0119] Table 3

[0120]

[0121]

[0122] From Table 1 to Table 3, we can see that:

[0123] It can be seen from Example 1 and Comparative Examples 1-3 that the manganese-zinc ferrite material obtained by the present invention has the characteristics of high magnetic permeability, wide frequency, wide temperature and low temperature coefficient. In the temperature range of 0-120°C, the magnetic permeability remains at a high level, and it also has a high Curie temperature, and the magnetic permeability does not drop at 300KHz; It can be seen from Example 1 and Comparative Example 4 that the present invention is coated with CaO, which can improve the resistivity of the product and improve the frequency characteristics by cooperating with the sintering process. Without adding calcium oxide, the magnetic permeability will increase, but the frequency characteristics will deteriorate; It can be seen from Example 1 and Example 5 that the auxiliary component of the present invention preferably also contains CaCO3; It can be seen from Example 1 and Example 6 that the auxiliary component of the present invention preferably contains CoO, and the use of Co 2+ The K1 value contributed by the ions drops sharply with the increase of temperature, which improves the material properties. If CoO is not added, the temperature characteristics will deteriorate. It can be seen from Examples 1 and 7 that the present invention preferably uses a main component and a nano-CaO mixture to achieve the coating of the main component, thereby promoting its role, otherwise the frequency characteristics will deteriorate. It can be seen from Examples 1 and 8 that the present invention first sintered at a low temperature and then sintered at a high temperature to achieve gradient sintering, and cooperated with the coating to achieve a broadband process, thereby improving the material properties. Otherwise, the overall grains will be larger and the frequency characteristics will deteriorate.

[0124] In summary, the present invention provides a manganese-zinc ferrite material and a preparation method and application thereof. The manganese-zinc ferrite material has high frequency, high magnetic permeability, high Curie temperature and low temperature coefficient characteristics through component combination, thereby realizing stable operation of the manganese-zinc ferrite material in the temperature range of 0-120°C in the electronic field.

[0125] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A manganese-zinc ferrite material, characterized in that: The manganese-zinc ferrite material comprises a main component, an additive and an auxiliary component, wherein the main component comprises 50.5-52.5 mol % of Fe2O3, 17.0-19.5 mol % of ZnO, and the balance is MnO; The additive includes CaO; The auxiliary components include Bi2O3 and MoO, or include CoO, Bi2O3 and MoO.

2. The manganese-zinc ferrite material according to claim 1, characterized in that: The main components include 50.5-52.5 mol% of Fe2O3, 17.0-19.5 mol% of ZnO and 30-30.5 mol% of MnO; Preferably, based on 100% of the total weight of the main components, the content of CaO is 400-2000 ppm.

3. The manganese-zinc ferrite material according to claim 1 or 2, characterized in that: Based on the total weight of the main component being 100%, the auxiliary component includes 0-2000 ppm of CoO, 200-2000 ppm of Bi2O3 and 200-2000 ppm of MoO; Preferably, based on 100% of the total weight of the main component, the auxiliary component further comprises 200-2000 ppm of CaCO3.

4. The manganese-zinc ferrite material according to any one of claims 1 to 3, characterized in that: The manganese-zinc ferrite material has a magnetic permeability μ i All are in the range of 10,000-11,000; Preferably, the Curie temperature of the manganese-zinc ferrite material is ≥150°C; Preferably, the manganese-zinc ferrite material has a magnetic permeability μ at 300 KHz. i ≥9500.

5. A method for preparing the manganese-zinc ferrite material according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) mixing and pre-calcining the main component and the additive to obtain a pre-calcined material; (2) mixing the auxiliary components with the pre-burned material in step (1) to obtain a mixed material; (3) tempering the mixed material in step (2) to obtain a tempered material; (4) mixing the binder with the tempered material in step (3) and granulating the mixture to obtain a granular material; (5) Pressing the granular material in step (4) into a shape, and then sintering it to obtain the manganese-zinc ferrite material.

6. The preparation method according to claim 5, characterized in that: The pre-burning temperature in step (1) is 700-800° C. and the time is 2-3 hours; Preferably, the mixing method in step (1) comprises ball milling.

7. The preparation method according to claim 5 or 6, characterized in that: The mixing method in step (2) includes sand milling and / or ball milling; Preferably, the tempering temperature in step (3) is 700-850°C.

8. The preparation method according to any one of claims 5 to 7, characterized in that: The amount of the binder added in step (4) is 5-10wt% of the tempering material in step (3), preferably 7-9wt%; Preferably, the sintering in step (5) is carried out in a protective gas, wherein the oxygen content in the protective gas is 3-21 vol%; Preferably, the sintering in step (5) includes first keeping the temperature at 600-700°C for 1-5h in a protective gas with an oxygen content of 19-21vol%, then heating to 1000-1100°C for 4-8h, and finally keeping the temperature at 1250-1360°C for 5-7h in a protective gas with an oxygen content of 3-7vol%.

9. The preparation method according to any one of claims 5 to 8, characterized in that: The preparation method comprises the following steps: (1) After the main component and CaO are ball-milled and dried, they are pre-fired at 700-800° C. for 2-3 hours in an air atmosphere to obtain a pre-fired material; (2) sand-milling and ball-milling the auxiliary components and the pre-burned material in step (1), and drying to obtain a mixed material; (3) tempering the mixed material in step (2) at 700-850° C. to obtain a tempered material; (4) mixing the tempered material of step (3) with 7-9 wt % of a binder and granulating the mixture to obtain a granular material; (5) Pressing the granular material prepared in step (4) into a mold, firstly keeping the temperature at 600-700° C. for 1-5 h in a protective gas with an oxygen content of 19-21 vol%, then heating the temperature to 1000-1100° C. for 4-8 h, and finally keeping the temperature at 1250-1360° C. for 5-7 h in a protective gas with an oxygen content of 3-7 vol%, to obtain the manganese-zinc ferrite material.

10. An application of the manganese-zinc ferrite material according to any one of claims 1 to 4, characterized in that: The applications include use in the field of automotive electronics.

Citation Information

Patent Citations

  • Low dissipative ferrite material of manganese and zinc in broad frequency, and high magnetic permeability, and preparation method

    CN101050108A

  • High-permeability manganese zinc ferrite material for automotive electronics and preparation method of material

    CN106747396A

Cited By

  • Manganese zinc ferrite material as well as preparation method and application thereof

    CN120794604A

  • High-permeability and high-impedance manganese zinc ferrite material for high frequency and preparation method thereof

    CN121913773A