YIG ferrite with high saturation flux density as well as preparation method and application of YIG ferrite

Through plasma-assisted ball milling technology, the sintering temperature is reduced and the press molding of polyvinyl alcohol aqueous solution is solved, and the shortcomings of existing ferrite materials in high magnetic field strength and microstructure manufacturing are prepared, and YIG ferrous oxygen with high saturation magnetic induction strength are prepared. , which meets the needs of radar, base station and other equipment.

CN118908710AActive Publication Date: 2024-11-08TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410951732.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing ferrite materials have shortcomings in high magnetic field strength and microstructure manufacturing, which are difficult to meet the needs of non-electronic systems such as radars, base stations and mobile phones. In particular, the internal electronic movement of garnet ferrite leads to magnetic permeability and magnetism. Insufficient saturation intensity.

Method used

By using plasma-assisted ball milling technology, YIG ferrite with small grains and high saturation magnetic induction strength is prepared by reducing the sintering temperature, and the first plasma-assisted ball milling is performed by mixing oxide powder, combining with polyvinyl alcohol aqueous solution. The press molding achieves efficient sintering treatment.

Benefits of technology

It effectively reduces the optimal phase formation temperature of YIG ferrite, significantly reduces the particle size and grain size of ferrite powder, improves its dielectric constant and saturated magnetic induction strength, and improves magnetic performance and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908710A_ABST
    Figure CN118908710A_ABST
Patent Text Reader

Abstract

The invention discloses YIG ferrite with high saturation flux density and a preparation method and application thereof, and belongs to the technical field of ferrite materials.The preparation method of the YIG ferrite with the high saturation flux density comprises the following steps that oxide mixed powder is subjected to plasma-assisted ball milling and drying, pretreated powder is obtained, sieving and presintering treatment are conducted, and the YIG ferrite with the high saturation flux density is obtained. And performing plasma-assisted ball milling and drying to obtain powder, mixing the powder with a polyvinyl alcohol aqueous solution, performing compression molding to obtain a ferrite green body, and performing sintering treatment to obtain the YIG ferrite. According to the preparation method disclosed by the invention, the optimal phase forming temperature of the YIG ferrite is reduced by plasma-assisted ball milling and sintering temperature reduction, the activity of the YIG ferrite is improved by changing the physical state of iron ions and exciting a chemical reaction through discharging, and the YIG ferrite with relatively high dielectric constant and high saturation flux density is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferrite materials, and in particular relates to a YIG ferrite with high saturation magnetic induction intensity and a preparation method and application thereof. Background Art

[0002] With the continuous development of wireless communication technology and network technology, wireless communication technology has rapidly entered people's daily life. The application of a large number of wireless communication technologies such as wireless networks and the Internet of Things has brought wireless communication technology into the 5G era. Microwave communication devices are devices used to process and transmit microwave frequency signals. They have been widely used in electronic equipment in various fields such as radar, communication, navigation, electronic countermeasures, satellite communications, radio and television, and microwave heating. Circulators and isolators are common electronic devices in microwave and radio frequency technology, and the magnetic materials used are usually ferrites. The difficulty of electron movement inside garnet ferrite makes it have relatively high magnetic permeability and magnetic saturation induction intensity, low electrical conductivity and loss, and good antioxidant properties and magnetic stability. In addition, there are three types of oxygen polyhedrons. By replacing the cations in the oxygen polyhedrons, their saturation magnetization, temperature stability, dielectric loss, coercivity and other properties can be appropriately adjusted to meet the needs of various applications.

[0003] At present, the demand for non-electronic systems such as radars, base stations and mobile phones has increased dramatically, which has driven the development and application of related components and also put forward higher requirements for ferrite materials. First of all, the ideal ferrite material should have sufficient saturation magnetization to ensure that it can withstand the required magnetic field strength in the circulator to achieve good magnetic properties. A higher saturation magnetization usually means that the material can reach saturation under a relatively small magnetic field, which helps to improve the magnetic properties and efficiency of the circulator. In addition, exploring new synthesis methods is also very important for improving the microstructure manufacturing, surface activity regulation and particle refinement of the material. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a YIG ferrite with high saturation magnetic induction intensity and its preparation method and application. By using plasma-assisted ball milling, YIG (garnet) ferrite with small grains and high saturation magnetic induction intensity is prepared at a lower sintering temperature.

[0005] To achieve the above object, the present invention provides a method for preparing YIG ferrite with high saturation magnetic induction intensity, comprising the following steps:

[0006] S1, the oxide mixed powder is first plasma-assisted ball milled and first dried to obtain a pretreated powder;

[0007] The pre-treated powders in S2 and S1 are screened, pre-sintered, subjected to a second plasma-assisted ball milling, and then dried to obtain a powder;

[0008] S3, the powder in step S2 is mixed with a polyvinyl alcohol aqueous solution, and pressed into a shape to obtain a ferrite green body;

[0009] S4, sintering the ferrite green body described in step S3 to obtain YIG ferrite.

[0010] Preferably, the proportion of the oxide mixed powder in step S1 is according to the chemical formula Y 2.7 Ca 0.3 Fe 4.5- x Sn 0.15 Zr 0.15 In 0.2 O 12-1.5x Calculation, wherein x is the iron deficiency, 0≤x≤1, and the purity of the oxide mixed powder is ≥99%.

[0011] Preferably, in step S1, the first plasma-assisted ball milling uses stainless steel balls as grinding media and deionized water as dispersant, the mass ratio of the oxide mixed powder, stainless steel balls and deionized water in the first plasma-assisted ball milling is 1:(4-6):(4-6), the rotation speed of the first plasma-assisted ball milling is 800-950 rad / min, and the effective time of the first plasma-assisted ball milling is 6-9h.

[0012] Preferably, the effective time of the first plasma ball milling in step S1 is the time for ball milling, and the procedure of the first plasma ball milling is ball milling for 30 minutes, pausing for 10 minutes, and cycling 12 times. The raw oxide mixed powder is mixed evenly through the first plasma ball milling so that the solid phase reaction is complete during pre-sintering.

[0013] Further preferably, the mass ratio of large, medium and small balls in the stainless steel balls is 2:5:3, the diameter of the big ball is 8 mm, the diameter of the medium ball is 5 mm, and the diameter of the small ball is 3 mm.

[0014] Preferably, in step S1, the temperature of the first drying is 80-100° C., and the time of the first drying is 10-12 hours.

[0015] Preferably, the aperture of the sieve in step S2 is 20-40 mesh; the pre-sintering temperature in step S2 is 1150-1300°C, and the pre-sintering time is 2-3h. After high-temperature treatment, the pre-treated powder after sieving undergoes a preliminary chemical reaction, and a part of it is converted into ferrite, so as to ensure that the microscopic morphology of the sintered sample is better, improve the sintering density, and reduce the product shrinkage rate; in step S2, the second plasma-assisted ball milling uses stainless steel balls as grinding media and deionized water as dispersant, and the mass ratio of the pre-treated powder after sieving, stainless steel balls and deionized water in the second plasma-assisted ball milling is 1:(4-6):(4-6), the rotation speed of the second plasma-assisted ball milling is 800-950rad / min, and the effective time of the second plasma-assisted ball milling is 6-9h; the temperature of the second drying in step S2 is 80-100°C, and the second drying time is 10-12h.

[0016] Preferably, the effective time of the second plasma ball milling in step S2 is the time for ball milling, and the procedure of the second plasma ball milling is ball milling for 30 minutes, pausing for 10 minutes, and repeating 12 times.

[0017] Preferably, the mixing mass ratio of the powder and the polyvinyl alcohol aqueous solution in step S3 is 1:(0.1-0.15); the concentration of the polyvinyl alcohol aqueous solution in step S3 is 5-7wt%; the pressing pressure in step S3 is 15-20Mpa, and the pressing time is 2-4min.

[0018] Preferably, the sintering temperature in step S4 is 1350-1480° C., and the sintering time is 3-5 hours.

[0019] The invention also provides the YIG ferrite prepared by the preparation method.

[0020] The present invention also provides the YIG ferrite prepared by the preparation method or the application of the YIG ferrite in preparing microwave and / or radio frequency electronic components.

[0021] Compared with the prior art, the present invention has the following advantages and technical effects:

[0022] The present invention uses oxide mixed powder as raw material, reduces the optimum phase forming temperature of YIG ferrite through plasma-assisted ball milling and lowering the sintering temperature, the particle size of ferrite powder after the first plasma-assisted ball milling and the second plasma-assisted ball milling is small, the grain size in the microstructure is significantly reduced, and the physical state of iron ions is changed by discharge and chemical reactions are stimulated to improve their activity, so as to prepare YIG ferrite with higher dielectric constant and high saturation magnetic induction intensity. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 X-ray diffraction patterns of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1;

[0025] Figure 2 hysteresis loop diagrams of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1;

[0026] Figure 3 This is a scanning electron microscope image of the YIG ferrite prepared in Example 1, with a scale of 15 μm;

[0027] Figure 4 This is a scanning electron microscope image of the YIG ferrite prepared in Comparative Example 1, with a scale of 15 μm;

[0028] Figure 5 The particle size diagrams of the YIG ferrite prepared in Example 1 after the first plasma-assisted ball milling and the second plasma-assisted ball milling, wherein A is the particle size diagram after the first plasma-assisted ball milling, and B is the particle size diagram after the second plasma-assisted ball milling;

[0029] Figure 6 The particle size diagrams of the YIG ferrite prepared in Comparative Example 1 after the first plasma-assisted ball milling and the second plasma-assisted ball milling, wherein A is the particle size diagram after the first plasma-assisted ball milling, and B is the particle size diagram after the second plasma-assisted ball milling;

[0030] Figure 7 The dielectric constant diagram of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1. DETAILED DESCRIPTION

[0031] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0032] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0033] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0034] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0035] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0036] Y2O3 powder was purchased from Shanghai McLean Biochemical Technology Co., Ltd., CaCO3 powder was purchased from Tianjin Oubokai Chemical Co., Ltd., SnO2 powder was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., ZrO2 powder was purchased from Tianjin Xiensi Biochemical Technology Co., Ltd., In2O3 powder was purchased from Shanghai McLean Biochemical Technology Co., Ltd., Fe2O3 powder was purchased from Tianjin Oubokai Chemical Co., Ltd., plasma ball mill was purchased from Guangzhou Huagong Optoelectronics Technology Co., Ltd., model PBM200, polyvinyl alcohol was purchased from Sinopharm Chemical Reagent Co., Ltd., and hydraulic sample making machine was purchased from Xiangtan Instrument Co., Ltd., model SDJ.

[0037] Example 1

[0038] S1, oxide mixed powder (the proportion of ingredients is according to the chemical formula Y 2.7 Ca 0.3 Fe 4.3 Sn 0.15 Zr 0.15 In 0.2 O 11.7Calculate, weigh Y2O3 powder, CaCO3 powder, SnO2 powder, ZrO2 powder, In2O3 powder, Fe2O3 powder) in proportion, load into plasma ball mill, use stainless steel ball as grinding medium, use deionized water as dispersant, rotate at 895rad / min, carry out first plasma assisted ball milling for 6h, ball milling mode is cyclic discharge, discharge frequency is 30.5KHz, discharge power is 15W, oxide mixed powder, stainless steel ball (large, medium and small ball diameters are 8mm, 5mm and 3mm respectively, and the mass ratio of large, medium and small balls is 2:5:3) and deionized water are mixed according to the mass ratio of 1:5:4, ball milling procedure is ball milling for 30min, pause for 10min, cycle 12 times, first drying at 100℃ for 10h, and obtain pretreated powder;

[0039] S2, the pretreated powder was sieved through a 30-mesh sieve, pre-sintered at 1200°C in a muffle furnace for 3h, and a second plasma-assisted ball milling was performed for 6h with stainless steel balls as grinding media and deionized water as dispersant at a speed of 895rad / min. The ball milling mode was cyclic discharge, the discharge frequency was 30.5KHz, and the discharge power was 15W. The sieved pretreated powder, stainless steel balls (the diameters of large, medium and small balls were 8mm, 5mm and 3mm respectively, and the mass ratio of large, medium and small balls was 2:5:3) and deionized water were mixed in a mass ratio of 1:5:4. The ball milling procedure was ball milling for 30min, pausing for 10min, circulating 12 times, and second drying at 100°C for 10h to obtain powder;

[0040] S3, the powder was mixed with a 5wt% polyvinyl alcohol aqueous solution at a mass ratio of 1:0.12, and the 5wt% polyvinyl alcohol aqueous solution was added dropwise while being manually ground, and then passed through a 40-mesh sieve, and 6.5g of the sieved powder was weighed, and pressed for 3min at a pressure of 18MPa using a hydraulic sample making machine to obtain a ferrite green body;

[0041] S4. The ferrite green body is placed in a muffle furnace for sintering treatment, and the procedure is: 20°C, heating to 150°C for 1h, keeping warm for 1h to drain, heating to 550°C for 2h, keeping warm for 1h to debind, sintering at 1400°C for 3h, keeping warm for 4h, then cooling to 500°C for 3h, and cooling naturally to obtain YIG ferrite.

[0042] Example 2

[0043] S1, oxide mixed powder (the proportion of ingredients is according to the chemical formula Y 2.7 Ca 0.3 Fe 4.3 Sn 0.15 Zr 0.15 In 0.2 O 11.7Calculate, weigh Y2O3 powder, CaCO3 powder, SnO2 powder, ZrO2 powder, In2O3 powder, Fe2O3 powder) in proportion, load into plasma ball mill, use stainless steel ball as grinding medium, use deionized water as dispersant, rotate at 800rad / min, carry out first plasma assisted ball milling for 6h, ball milling mode is cyclic discharge, discharge frequency is 30.5KHz, discharge power is 15W, oxide mixed powder, stainless steel ball (large, medium and small ball diameters are 8mm, 5mm and 3mm respectively, and the mass ratio of large, medium and small balls is 2:5:3) and deionized water are mixed according to the mass ratio of 1:4:5, the ball milling procedure is ball milling for 30min, pause for 10min, cycle 12 times, first drying at 80℃ for 12h, and obtain pretreated powder;

[0044] S2, the pretreated powder was sieved through a 20-mesh sieve, pre-sintered at 1150° C. in a muffle furnace for 3 h, and a second plasma-assisted ball milling was performed for 6 h using stainless steel balls as grinding media and deionized water as dispersant at a speed of 800 rad / min. The ball milling mode was cyclic discharge, the discharge frequency was 30.5 KHz, and the discharge power was 15 W. The sieved pretreated powder, stainless steel balls (the diameters of the large, medium and small balls were 8 mm, 5 mm and 3 mm, respectively, and the mass ratio of the large, medium and small balls was 2:5:3) and deionized water were mixed in a mass ratio of 1:6:6. The ball milling procedure was ball milling for 30 min, pausing for 10 min, circulating 12 times, and second drying at 80° C. for 12 h to obtain a powder;

[0045] S3, the powder was mixed with a 6wt% polyvinyl alcohol aqueous solution at a mass ratio of 1:0.1, and the 6wt% polyvinyl alcohol aqueous solution was added dropwise while being manually ground, and then passed through a 40-mesh sieve, and 6.5g of the sieved powder was weighed, and pressed for 4 minutes at a pressure of 15MPa using a hydraulic sample making machine to obtain a ferrite green body;

[0046] S4. The ferrite green body is placed in a muffle furnace for sintering treatment, and the procedure is: 20°C, heating to 150°C for 1h, keeping warm for 1h to drain, heating to 550°C for 2h, keeping warm for 1h to debind, sintering at 1350°C for 5h, keeping warm for 4h, then cooling to 500°C for 3h, and cooling naturally to obtain YIG ferrite.

[0047] Example 3

[0048] S1, oxide mixed powder (the proportion of ingredients is according to the chemical formula Y 2.7 Ca 0.3 Fe 4.3 Sn 0.15 Zr 0.15 In 0.2 O 11.7Calculate, weigh Y2O3 powder, CaCO3 powder, SnO2 powder, ZrO2 powder, In2O3 powder, Fe2O3 powder) in proportion, load into plasma ball mill, use stainless steel ball as grinding medium, use deionized water as dispersant, rotate at 950rad / min, carry out first plasma assisted ball milling for 6h, ball milling mode is cyclic discharge, discharge frequency is 30.5KHz, discharge power is 15W, oxide mixed powder, stainless steel ball (large, medium and small ball diameters are 8mm, 5mm and 3mm respectively, and the mass ratio of large, medium and small balls is 2:5:3) and deionized water are mixed according to the mass ratio of 1:5:5, the ball milling procedure is ball milling for 30min, pause for 10min, cycle 12 times, first drying at 90℃ for 11h, and obtain pretreated powder;

[0049] S2, the pretreated powder was sieved through a 40-mesh sieve, pre-sintered at 1300°C in a muffle furnace for 2h, and stainless steel balls were used as grinding media, deionized water was used as a dispersant, and the rotation speed was 950rad / min. The second plasma-assisted ball milling was performed for 6h. The ball milling mode was cyclic discharge, the discharge frequency was 30.5KHz, and the discharge power was 15W. The sieved pretreated powder, stainless steel balls (the diameters of large, medium and small balls were 8mm, 5mm and 3mm respectively, and the mass ratio of large, medium and small balls was 2:5:3) and deionized water were mixed according to the mass ratio of 1:5:6. The ball milling procedure was ball milling for 30min, pausing for 10min, circulating 12 times, and second drying at 90°C for 11h to obtain powder;

[0050] S3, the powder was mixed with a 7wt% polyvinyl alcohol aqueous solution at a mass ratio of 1:0.15, and the 7wt% polyvinyl alcohol aqueous solution was added dropwise while being manually ground, and then passed through a 40-mesh sieve, and 6.5g of the sieved powder was weighed, and pressed for 2min at a pressure of 20MPa using a hydraulic sample making machine to obtain a ferrite green body;

[0051] S4. The ferrite green body is placed in a muffle furnace for sintering treatment, and the procedure is: 20°C, heating to 150°C for 1h, keeping warm for 1h to drain, heating to 550°C for 2h, keeping warm for 1h to debind, sintering at 1480°C for 3h, keeping warm for 4h, then cooling to 500°C for 3h, and cooling naturally to obtain YIG ferrite.

[0052] Comparative Example 1

[0053] S1, oxide mixed powder (the proportion of ingredients is according to the chemical formula Y 2.7 Ca 0.3 Fe 4.3 Sn 0.15 Zr 0.15 In 0.2 O 11.7Calculate, weigh Y2O3 powder, CaCO3 powder, SnO2 powder, ZrO2 powder, In2O3 powder, Fe2O3 powder) in proportion, load into plasma ball mill, use stainless steel ball as grinding medium, use deionized water as dispersant, rotate at 895rad / min, carry out first plasma-assisted ball milling for 6h, ball milling mode is cyclic vibration, oxide mixed powder, stainless steel ball (large, medium and small ball diameters are 8mm, 5mm and 3mm respectively, and the mass ratio of large, medium and small balls is 2:5:3) and deionized water are mixed in a mass ratio of 1:5:4, ball milling procedure is ball milling for 30min, pause for 10min, cycle 12 times, first drying at 100℃ for 12h, and obtain pretreated powder;

[0054] S2, the pretreated powder was sieved through a 30-mesh sieve, pre-sintered at 1250° C. in a muffle furnace for 3 h, and a second plasma-assisted ball milling was performed for 6 h at a speed of 895 rad / min using stainless steel balls as grinding media and deionized water as dispersant. The ball milling mode was cyclic vibration, and the sieved pretreated powder, stainless steel balls (the diameters of large, medium and small balls were 8 mm, 5 mm and 3 mm, respectively, and the mass ratio of large, medium and small balls was 2:5:3) and deionized water were mixed in a mass ratio of 1:5:4. The ball milling procedure was ball milling for 30 min, pausing for 10 min, circulating 12 times, and second drying at 100° C. for 12 h to obtain a powder;

[0055] S3, the powder was mixed with a 5wt% polyvinyl alcohol aqueous solution at a mass ratio of 1:0.12, and the 5wt% polyvinyl alcohol aqueous solution was added dropwise while being manually ground, and then passed through a 40-mesh sieve, and 6.5g of the sieved powder was weighed, and pressed for 3min at a pressure of 18MPa using a hydraulic sample making machine to obtain a ferrite green body;

[0056] S4. The ferrite green body is placed in a muffle furnace for sintering treatment, and the procedure is: 20°C, heating to 150°C for 1h, keeping warm for 1h to drain, heating to 550°C for 2h, keeping warm for 1h to debind, sintering at 1450°C for 3h, keeping warm for 4h, then cooling to 500°C for 3h, and cooling naturally to obtain YIG ferrite.

[0057] Experimental example

[0058] The X-ray diffraction patterns of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1 were measured by an X-ray diffractometer (SmartLsbSE, JpanRIGAKUCORPORATION), which used CuKa rays, a step size of 0.01° within 2θ, a scanning rate of 10 (°) / min, and recorded Xrd spectra in the 2θ range of 20° to 80°.

[0059] The hysteresis loops of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1 were measured; the saturated applied magnetic field strength was 1590 A / m as tested by a soft magnetic DC test system (TS4000, Tunkia Co.).

[0060] The scanning electron microscope images of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1 were measured; a scanning electron microscope (JSM-7900F, Japan) was used with a voltage of 15 kV, a magnification of 8500x, and a scale of 15 μm.

[0061] The particle size diagram after plasma-assisted ball milling of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1 was measured by a laser particle size analyzer (BT-9000ST, Dandong Better Instrument Co., Ltd.), the material selected was ferric oxide, and the medium was water.

[0062] The dielectric constant diagrams of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1 were measured by a vector network analyzer (VNA, ZNA43, Rohde & Schwarz, Germany) using a coaxial method.

[0063] like Figure 1 The Xrd spectra of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1 are shown in FIG. 12 Compared with the PDF standard card, no impurity peaks were generated, and a single garnet phase was formed.

[0064] like Figure 2 As shown, it is the hysteresis loop diagram of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1. Through plasma-assisted ball milling, the saturation magnetic induction intensity and the residual magnetic induction intensity of the YIG ferrite prepared in Example 1 are greater than those of the YIG ferrite prepared in Comparative Example 1, and the magnetic properties are better.

[0065] like Figure 3 As shown, it is a scanning electron microscope image of the YIG ferrite prepared in Example 1. Figure 4 , which is a scanning electron microscope image of the YIG ferrite prepared in Comparative Example 1. Under the same magnification and scale, the grain size of the YIG ferrite prepared in Example 1 through plasma-assisted ball milling is significantly smaller than that of Comparative Example 1.

[0066] like Figure 5 As shown, Figure 5 A is the particle size diagram of the YIG ferrite prepared in Example 1 after the first ball milling. Figure 5 B is the particle size diagram of the YIG ferrite prepared in Example 1 after the second ball milling. The particle size of the powder obtained by the second ball milling becomes smaller, such as Figure 6 As shown, Figure 6A is the particle size diagram of the YIG ferrite prepared in Comparative Example 1 after one ball milling. Figure 6 B is a particle size diagram of the YIG ferrite prepared in Comparative Example 1 after secondary ball milling. Through plasma-assisted ball milling, the powder particle size of the YIG ferrite of Example 1 after each ball milling is smaller than that of the YIG ferrite of Comparative Example 1, and a finer powder can be obtained.

[0067] like Figure 7 As shown, it is a diagram of the dielectric constants of the YIG ferrite prepared in Example 1 and the YIG ferrite prepared in Comparative Example 1 at 2 to 8 GHz. The dielectric properties of the YIG ferrite prepared in Example 1 are better than those of the YIG ferrite prepared in Comparative Example 1. The dielectric constant of YIG is about 14.5, and its dielectric constant can be improved by plasma-assisted ball milling.

[0068] Table 1 Comparison of ferrite data prepared in Example 1 and Comparative Example 1

[0069] Group Components Is it single phase? Ball milling method Sintering temperature Bs(Gs) Example 1 <![CDATA[Y 2.7 Ca 0.3 Fe 4.3 Sn 0.15 Zr 0.15 In 0.2 O 11.7 ]]> yes Cyclic discharge 1400℃ 1887 Comparative Example 1 <![CDATA[Y 2.7 Ca 0.3 Fe 4.3 Sn 0.15 Zr 0.15 In 0.2 O 11.7 ]]> yes Cyclic vibration 1450℃ 1736

[0070] It can be seen from Table 1 that the magnetic properties of the YIG ferrite obtained by plasma-assisted ball milling in Example 1 are better than those of the YIG ferrite obtained by traditional ball milling in Comparative Example 1, and the optimal sintering temperature is reduced.

[0071] In summary, the preparation method of the present invention reduces the optimal phase formation temperature of garnet ferrite through plasma-assisted ball milling. After the first and second grindings, the particle size of the ferrite powder is small, and the grain size in the microstructure is significantly reduced. The physical state of iron ions is changed by discharge and chemical reactions are stimulated to increase their activity, thereby preparing YIG ferrite with a higher dielectric constant and a high saturation magnetic induction intensity.

[0072] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing YIG ferrite with high saturation magnetic induction intensity, characterized in that: The following steps are involved: S1, the oxide mixed powder is first plasma-assisted ball milled and first dried to obtain a pretreated powder; The pre-treated powders in S2 and S1 are screened, pre-sintered, subjected to a second plasma-assisted ball milling, and then dried to obtain a powder; S3, the powder in step S2 is mixed with a polyvinyl alcohol aqueous solution, and pressed into a shape to obtain a ferrite green body; S4, sintering the ferrite green body described in step S3 to obtain YIG ferrite.

2. The preparation method according to claim 1, characterized in that: The proportion of the oxide mixed powder in step S1 is based on the chemical formula Y 2.7 Ca 0.3 Fe 4.5-x Sn 0.15 Zr 0.15 In 0.2 O 12-1.5x Calculation, wherein x is the iron deficiency, 0≤x≤1, and the purity of the oxide mixed powder is ≥99%.

3. The preparation method according to claim 1, characterized in that: In step S1, the first plasma-assisted ball milling uses stainless steel balls as grinding media and deionized water as dispersant. The mass ratio of the oxide mixed powder, stainless steel balls and deionized water in the first plasma-assisted ball milling is 1:(4-6):(4-6). The rotation speed of the first plasma-assisted ball milling is 800-950 rad / min. The effective time of the first plasma-assisted ball milling is 6-9 hours.

4. The preparation method according to claim 3, characterized in that: The mass ratio of large, medium and small balls in the stainless steel balls is 2:5:

3.

5. The preparation method according to claim 1, characterized in that: In step S1, the temperature of the first drying is 80-100° C., and the time of the first drying is 10-12 hours.

6. The preparation method according to claim 1, characterized in that: The aperture of the sieve in step S2 is 20 to 40 meshes; the temperature of the pre-sintering in step S2 is 1150 to 1300° C., and the time of the pre-sintering is 2 to 3 hours; in step S2, the second plasma-assisted ball milling uses stainless steel balls as grinding media and deionized water as dispersant, and the mass ratio of the sieved pretreated powder, stainless steel balls and deionized water in the second plasma-assisted ball milling is 1:(4 to 6):(4 to 6), the rotation speed of the second plasma-assisted ball milling is 800 to 950 rad / min, and the effective time of the second plasma-assisted ball milling is 6 to 9 hours; in step S2, the temperature of the second drying is 80 to 100° C., and the time of the second drying is 10 to 12 hours.

7. The preparation method according to claim 1, characterized in that: The mixing mass ratio of the powder and the polyvinyl alcohol aqueous solution in step S3 is 1:(0.1-0.15); the concentration of the polyvinyl alcohol aqueous solution in step S3 is 5-7wt%; the pressing pressure in step S3 is 15-20Mpa, and the pressing time is 2-4min.

8. The preparation method according to claim 1, characterized in that: The sintering temperature in step S4 is 1350-1480° C., and the sintering time is 3-5 hours.

9. The YIG ferrite prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the YIG ferrite prepared by the preparation method according to any one of claims 1 to 8 or the YIG ferrite according to claim 9 in the preparation of microwave and / or radio frequency electronic components.

Citation Information

Patent Citations

  • Manganese-zinc ferrite pre-sintering material and preparation process thereof

    CN112723872A

  • Superfine rare earth soft magnetic material and preparation method and application thereof

    CN115966395A

  • Ferrite circulator substrate with self-bias effect and preparation method and application thereof

    CN117937084A

  • Thermoelectric conversion material

    JP2014225655A

  • Semiconductor Device and Method of Forming Hybrid Substrate with Uniform Thickness

    US20240071885A1