Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high-temperature piezoelectric ceramic material and preparation method thereof
High-temperature piezoelectric ceramic materials were prepared by Na/Sr/Ce/Cr/Ta/Mo doping modification and spark plasma sintering technology, which solved the problems of depolarization and environmental pollution of lead zirconate titanate piezoelectric ceramics at high temperatures, and realized CaBi2Nb2O9 materials with high Curie temperature and excellent piezoelectric properties.
Patent Information
- Application Number
- CN202410976056.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing lead zirconate titanate piezoelectric ceramic materials suffer from severe depolarization at high temperatures, have low Curie temperatures, and contain lead which is harmful to the environment, making it difficult to maintain excellent piezoelectric performance in high-temperature environments.
The CaBi₂Nb₂O₉ material was modified by using Na/Sr/Ce/Cr/Ta/Mo doping ions. High-temperature piezoelectric ceramics were prepared by doping [Na₀.₂Sr₀.₄Ce₀.₄]²⁶⁺ ions at the A site and [Cr₀.₅Ta₀.₃Mo₀.₆₅]₅₅⁺ ions at the B site, combined with spark plasma sintering technology.
The material exhibits improved piezoelectric properties and high-temperature stability, with a Curie temperature exceeding 900℃, a piezoelectric constant d33 ≥ 21.5 pC/N, and low dielectric loss, making it suitable for sensors, transducers, and other components in high-temperature environments.
Smart Images

Figure CN118908716A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piezoelectric ceramic materials, and in particular to a method for preparing a doped bismuth layered structure calcium bismuth niobate high-temperature piezoelectric ceramic material. Background Art
[0002] At present, the most widely used piezoelectric ceramic material is mainly lead zirconate titanate piezoelectric ceramics, but this type of piezoelectric ceramics contains lead, which causes harm to the environment and human body during production, use and waste disposal, and the Curie temperature of this type of piezoelectric ceramics is generally below 400℃. Due to the existence of the depolarization phenomenon of piezoelectric materials, piezoelectric materials cannot work normally above the Curie temperature. With the rapid development of aerospace, geological exploration and other work and in line with the needs of sustainable development of human society, it is necessary to seek an environmentally friendly piezoelectric material with high Curie temperature and excellent piezoelectric performance.
[0003] Bismuth layered ceramics have the characteristics of high Curie temperature, low dielectric loss, obvious anisotropy of electromechanical coupling coefficient, high resistivity, no pollution, low leakage current, excellent ferroelectric properties, etc., and are candidate materials suitable for high temperature environments. Bismuth layered ceramic materials are composed of (Bi2O2) 2+ The layers and perovskite structure lattice layers are alternately stacked, and its chemical formula is (Bi2O2) 2+ (A m-1 B m O 3m+1 ) 2- Among them, CaBi2Nb2O9 (CBN) is a typical bismuth layered structure ferroelectric material, A is a 12-coordinated Ca 2+ , B is 6-coordinated Nb 5+ , m = 2, fluorite structure (Bi2O2) 2+ The Curie temperature (T C ≈943℃) is the highest among bismuth layered ceramics, but the piezoelectric constant is very low (d 33 ≈6pC / N). Therefore, how to maintain a high Curie temperature while improving the piezoelectric activity and obtaining CBN piezoelectric ceramic materials with excellent comprehensive electrical properties has become an important research topic in the field of high-temperature piezoelectric ceramic materials. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material. 2+ ions, using K with 12 coordination + , Ba 2+ , Y 3+Composition of complex high-valent ions [Na 0.2 Sr 0.4 Ce 0.4 ] 2.6+ Doping substitution is performed for Nb at the B position 5+ ions, using Cr with 6 coordination 2+ 、 5+ 、Mo 6+ Composition of complex high-valent ions [Cr 0.05 Ta 0.3 Mo 0.65 ] 5.5+ Doping substitution is performed so that through the above-mentioned composite doping modification, the piezoelectric properties and high-temperature resistivity are improved while maintaining a high Curie temperature, thereby providing a new type of environmentally friendly piezoelectric ceramic material with excellent comprehensive electrical properties. Another object of the present invention is to provide a method for preparing the above-mentioned Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high-temperature piezoelectric ceramic material.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] The present invention provides a Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material with a 12-coordinated K + , Ba 2+ , Y 3+ The complex high-valent ions [Na 0.2 Sr 0.4 Ce 0.4 ] 2.6+ Doping to replace Ca at the A position in CaBi2Nb2O9 2+ ions, with Cr having 6 coordination 2+ 、 5+ 、Mo 6+ The complex high-valent ions [Cr 0.05 Ta 0.3 Mo 0.65 ] 5.5+ Doping with Nb to replace the B site in CaBi2Nb2O9 5+ ions, the chemical formula is Ca 1-x [Na 0.2 Sr 0.4 Ce 0.4 ] x Bi 2-y [Cr 0.05 Ta 0.3 Mo 0.65 ] y O9, where 0.015≤x≤0.045, 0.025≤y≤0.06.
[0007] In the above scheme, the piezoelectric ceramic material of the present invention has a 33 ≥21.5pC / N, T C ≥900℃; Resistivity (ρ) ≥4.2×10 at 500℃ 8 Ω·cm, dielectric loss (tanδ) ≤ 0.20%; d after annealing at 800℃ 33 ≥18.2pC / N.
[0008] Another object of the present invention is achieved by the following technical solutions:
[0009] The method for preparing the above-mentioned Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material provided by the present invention comprises the following steps:
[0010] (1) Preparation of pre-synthesized precursor powder
[0011] CaCO3, Na2CO3, SrCO3, CeO2, Bi2O3, Nb2O5, Cr2O3, Ta2O5 and MoO3 are used as raw materials corresponding to Ca, Na, Sr, Ce, Bi, Nb, Cr, Ta and Mo in the chemical formula; each raw material is prepared according to the stoichiometric amount in the chemical formula, and then a ball milling treatment is carried out using anhydrous ethanol as a ball milling medium, and the obtained material is dried, sieved and pressed into shape, and then placed in a sealed crucible for calcination treatment; then the calcined material is ground and sieved, and a second ball milling treatment is carried out, and the obtained material is dried, ground and sieved to obtain a pre-synthesized precursor powder;
[0012] (2) Preparation of high temperature piezoelectric ceramic materials
[0013] The pre-synthesized precursor powder is loaded into a graphite mold, and placed in a spark plasma sintering furnace for a calcination treatment to obtain a carbon-containing sintered product; then the carbon-containing sintered product is placed in an ordinary high-temperature furnace under an air atmosphere for a secondary calcination treatment to decarbonize, thereby obtaining a decarbonized sintered product; finally, the decarbonized sintered product is polarized to obtain a high-temperature piezoelectric ceramic material.
[0014] Furthermore, in the step (1) of the preparation method of the present invention, the pressure of the pressing molding is 4-6 MPa; the calcination treatment is to increase the temperature to 830-880° C. at 5° C. / min and keep the temperature for 3-5 hours.
[0015] Furthermore, in the first calcination treatment in step (2) of the preparation method of the present invention, the spark plasma sintering furnace pressure is 40-45MPa, the DC pulse current is 600-650A, the temperature is first increased to 900°C at 100°C / min, then increased to 950-1000°C at 20°C / min, kept warm for 5-6min, cooled to 600°C at a cooling rate of 50°C / min, the DC pulse current is stopped, and then the pressure is released and the furnace is cooled to room temperature; the second calcination treatment is increased to 700-750°C at 5°C / min, kept warm for 4-4.5h, and cooled to room temperature with the furnace.
[0016] In the above scheme, the polarization treatment in step (2) of the preparation method of the present invention is to first polish the surface of the decarbonized sintered product; then perform electrode coating treatment, that is, silver electrodes are applied to the upper and lower surfaces of the decarbonized sintered product after polishing; then increase the temperature to 700-800°C at 5°C / min for calcination, keep warm for 20-30 minutes, and cool to room temperature with the furnace; finally, polarize in high-temperature silicone oil at 180-200°C with a DC voltage of 10-15kV / mm for polarization for 25-35 minutes.
[0017] The product is made using the above-mentioned method for preparing Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high-temperature piezoelectric ceramic material.
[0018] The present invention has the following beneficial effects:
[0019] (1) In the process of preparing CaBi2Nb2O9 piezoelectric ceramic materials, bismuth vacancies are inevitably formed due to the volatilization of bismuth at high temperature, thereby generating vacancy defects. In view of this phenomenon, the present invention adopts a valence ratio of Ca2O9 at the A site. 2+ Ions with high complex high valence [Na 0.2 Sr 0.4 Ce 0.4 ] 2.6+ Doping and substitution are performed to increase the mixing entropy of the material. 5+ Ionic high complex ions [Cr 0.05 Ta 0.3 Mo 0.65 ] 5.5+ Doping and substitution are performed to make the A and B positions both defective, making the perovskite layer (A m-1 B m O 3m+1 ) 2- Generates electrons, thereby strengthening the bismuth oxide layer (Bi2O2) 2+ and perovskite-like layers (A m-1 B m O 3m+1 ) 2-The interaction between them can then regulate the growth behavior of the grains, causing them to locally produce polarized nanodomains, and ultimately obtaining the CaBi2Nb2O9 high-temperature piezoelectric ceramic material with excellent performance.
[0020] (2) The present invention adopts advanced spark plasma sintering technology, which requires low sintering temperature and short time, thus low energy consumption, and high density of the material after sintering, thereby obtaining CaBi2Nb2O9 high-temperature piezoelectric ceramic materials with excellent performance.
[0021] (3) The piezoelectric ceramic material of the present invention, which is doped with Na, Sr, Ce at the Ca position and Cr, Ta, Mo at the Nb position, has a Curie temperature above 900°C and a piezoelectric constant d 33 ≥21.5pC / N, d after annealing at 800℃ 33 ≥18.2pC / N; resistivity ≥4.2×10 at 500℃ 8 Ω·cm, dielectric loss ≤0.20%. The material has good high temperature stability and can fully meet the application requirements of piezoelectric ceramic sensors, transducers, brakes and other components in high temperature environments, and has broad application prospects in high temperature electronic equipment.
[0022] (4) The preparation method of the present invention adopts advanced ceramic preparation technology, has low firing temperature, low preparation cost, simple and easy process operation, and easy control of influencing factors. It is suitable for large-scale industrial production and is conducive to promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings:
[0024] Figure 1 is the XRD crystal phase spectrum of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples;
[0025] Figure 2 is the piezoelectric constant d of the piezoelectric ceramic materials of the embodiment of the present invention and the comparative example 33 Curves changing with temperature. DETAILED DESCRIPTION
[0026] Embodiment 1:
[0027] This embodiment provides a method for preparing a Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material. The chemical formula of the piezoelectric ceramic material is Ca 1.96 [Na 0.2 Sr 0.4 Ce 0.4 ] 0.04 Bi 1.97 [Cr 0.05 Ta0.3 Mo 0.65 ] 0.03 O9, the preparation method has the following steps:
[0028] (1) Preparation of pre-synthesized precursor powder
[0029] CaCO3, Na2CO3, SrCO3, CeO2, Bi2O3, Nb2O5, Cr2O3, Ta2O5 and MoO3 with a purity of 99.9% are used as raw materials corresponding to Ca, Na, Sr, Ce, Bi, Nb, Cr, Ta and Mo in the above chemical formula. Each raw material is mixed according to the stoichiometric amount in the above chemical formula, and then anhydrous ethanol is used as the ball milling medium, according to the ratio of balls: material: anhydrous ethanol = 4:1:3, and the speed is 400r / min for a first ball milling treatment on a planetary ball mill for 24 hours, the obtained material is dried, sieved through an 80-mesh sieve, pressed and formed at 4 MPa, placed in a sealed crucible, and heated to 830°C at a rate of 5°C / min for calcination in an oxidizing atmosphere for 5 hours; the calcined material is ground and sieved through an 80-mesh sieve, and a second ball milling treatment is performed using the same process as the first ball milling treatment, and the obtained material is dried, ground, and sieved through an 80-mesh sieve to obtain a pre-synthesized precursor powder;
[0030] (2) Preparation of high temperature piezoelectric ceramic materials
[0031] (2-1) 0.8 g of the above-mentioned pre-synthesized precursor powder was loaded into a cylindrical graphite mold with a diameter of 20 mm, and placed in a spark plasma sintering furnace. The pressure was set to 44 MPa and the DC pulse current was set to 640 A. The temperature was first increased to 900° C. at 100° C. / min, and then increased to 960° C. at 20° C. / min. A calcination treatment was performed. After keeping the temperature for 6 minutes, the temperature was reduced to 600° C. at a cooling rate of 50° C. / min. The DC pulse current was stopped, and then the pressure was released. The product was cooled to room temperature in the furnace to obtain a carbon-containing sintered product.
[0032] (2-2) placing the carbon-containing sintered product in a common high-temperature furnace, and performing secondary calcination treatment at a temperature of 5°C / min to 750°C in an air atmosphere to decarbonize the product, keeping the temperature for 4 hours, and cooling the product to room temperature to obtain a decarbonized sintered product;
[0033] (2-3) The decarburized sintered product is subjected to the following polarization treatment: first, the surface of the decarburized sintered product is polished; then, electrode coating is performed, i.e., silver electrodes are applied to the upper and lower surfaces of the decarburized sintered product after polishing; then, the temperature is raised to 800°C at a rate of 5°C / min, kept at that temperature for 20 minutes, and cooled to room temperature with the furnace; finally, polarization is performed in high-temperature silicone oil at 180°C with a DC voltage of 10 to 15 kV / mm for 25 minutes, thereby obtaining a high-temperature piezoelectric ceramic material.
[0034] Embodiment 2:
[0035] The present embodiment is a method for preparing a Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material, which is different from the first embodiment in that:
[0036] 1. The general chemical formula of this embodiment is Ca 1.97 [Na 0.2 Sr 0.4 Ce 0.4 ] 0.03 Bi 1.95 [Cr 0.05 Ta 0.3 Mo 0.65 ] 0.05 O9.
[0037] 2. The calcination temperature in step (1) is 860°C and the holding time is 4h.
[0038] 3. The calcination system in step (2-1) is as follows: the pressure is set to 42 MPa and the DC pulse current is set to 620 A. The temperature is first raised to 900 ° C at 100 ° C / min, and then raised to 980 ° C at 20 ° C / min. A calcination treatment is performed. After keeping the temperature for 5 minutes, the temperature is reduced to 600 ° C at a cooling rate of 50 ° C / min, the DC pulse current is stopped, and then the pressure is released. The product is cooled to room temperature in the furnace to obtain a carbon-containing sintered product.
[0039] Embodiment three:
[0040] The present embodiment is a method for preparing a Na / Ba / Nd / Ga / Sb / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material, which is different from the first embodiment in that:
[0041] 1. The general chemical formula of this embodiment is Ca 1.98 [Na 0.2 Sr 0.4 Ce 0.4 ] 0.02 Bi 1.94 [Cr 0.05 Ta 0.3 Mo 0.65 ] 0.06 O9.
[0042] 2. The calcination temperature in step (1) is 880°C and the holding time is 3.5h.
[0043] 3. The calcination system in step (2-1) is as follows: the pressure is set to 42 MPa and the DC pulse current is set to 620 A. The temperature is first raised to 900 ° C at 100 ° C / min, and then raised to 950 ° C at 20 ° C / min. A calcination treatment is carried out. After keeping the temperature for 5 minutes, the temperature is reduced to 600 ° C at a cooling rate of 50 ° C / min, the DC pulse current is stopped, and then the pressure is released. The product is cooled to room temperature in the furnace to obtain a carbon-containing sintered product.
[0044] Comparative Example:
[0045] An undoped high temperature piezoelectric ceramic material with the general chemical formula of CaBi2Nb2O9 is used as a comparative example, and its preparation steps are the same as those in Example 1.
[0046] The XRD crystal phase spectra of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples are as follows: Figure 1 As shown, from Figure 1 It can be seen that the diffraction peaks of the piezoelectric ceramic materials prepared in the embodiments and comparative examples are completely consistent with the standard spectrum PDF 00-49-0608, indicating that the obtained materials are CaBi2Nb2O9 materials with a single crystal phase.
[0047] Piezoelectric constant d of piezoelectric ceramic materials in the embodiments of the present invention and the comparative examples 33 The temperature change curve is as follows Figure 2 As shown. Figure 2 It can be seen that from room temperature to 600°C, the d 33 The value decreases slightly with the increase of temperature. At 800℃, d 33 The value still remains above 85% of that at room temperature, indicating that the material has good temperature stability and is conducive to its application in high temperature fields.
[0048] The performance test results of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples are shown in Table 1.
[0049] Table 1 Properties of piezoelectric ceramic materials of the embodiments of the present invention and comparative examples
[0050]
Claims
1. A Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material, characterized in that: With 12-coordinate K + , Ba 2+ , Y 3+ The complex high-valent ions [Na 0.2 Sr 0.4 Ce 0.4 ] 2.6+ Doping to replace Ca at the A position in CaBi2Nb2O9 2+ ions, with Cr having 6 coordination 2+ 、 5+ 、Mo 6+ The complex high-valent ions [Cr 0.05 Ta 0.3 Mo 0.65 ] 5.5+ Doping with Nb to replace the B site in CaBi2Nb2O9 5+ ions, the chemical formula is Ca 1-x [Na 0.2 Sr 0.4 Ce 0.4 ] x Bi 2-y [Cr 0.05 Ta 0.3 Mo 0.65 ] y O9, where 0.015≤x≤0.045, 0.025≤y≤0.
06.
2. The Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material according to claim 1, characterized in that: The d of the piezoelectric ceramic material 33 ≥21.5pC / N, T C ≥900℃; Resistivity (ρ) ≥4.2×10 at 500℃ 8 Ω·cm, dielectric loss (tanδ) ≤ 0.20%; d after annealing at 800℃ 33 ≥18.2pC / N.
3. The method for preparing the Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material according to claim 1 or 2, characterized in that The following steps are involved: (1) Preparation of pre-synthesized precursor powder CaCO3, Na2CO3, SrCO3, CeO2, Bi2O3, Nb2O5, Cr2O3, Ta2O5 and MoO3 are used as raw materials corresponding to Ca, Na, Sr, Ce, Bi, Nb, Cr, Ta and Mo in the chemical formula; each raw material is prepared according to the stoichiometric amount in the chemical formula, and then a ball milling treatment is carried out using anhydrous ethanol as a ball milling medium, and the obtained material is dried, sieved and pressed into shape, and then placed in a sealed crucible for calcination treatment; then the calcined material is ground and sieved, and a second ball milling treatment is carried out, and the obtained material is dried, ground and sieved to obtain a pre-synthesized precursor powder; (2) Preparation of high temperature piezoelectric ceramic materials The pre-synthesized precursor powder is loaded into a graphite mold, and placed in a spark plasma sintering furnace for a calcination treatment to obtain a carbon-containing sintered product; then the carbon-containing sintered product is placed in an ordinary high-temperature furnace under an air atmosphere for a secondary calcination treatment to decarbonize, thereby obtaining a decarbonized sintered product; finally, the decarbonized sintered product is polarized to obtain a high-temperature piezoelectric ceramic material.
4. The method for preparing the Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material according to claim 3, characterized in that: The pressure of the pressing molding in the step (1) is 4-6 MPa; the calcination treatment is to increase the temperature to 830-880° C. at 5° C. / min and keep the temperature for 3-5 hours.
5. The method for preparing the Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material according to claim 3, characterized in that: The primary calcination treatment in step (2) is as follows: the spark plasma sintering furnace pressure is 40-45 MPa, the DC pulse current is 600-650A, the temperature is first raised to 900°C at 100°C / min, then raised to 950-1000°C at 20°C / min, kept at that temperature for 5-6 minutes, then cooled to 600°C at a cooling rate of 50°C / min, the DC pulse current is stopped, and then the pressure is released and the furnace is cooled to room temperature; the secondary calcination treatment is as follows: the temperature is raised to 700-750°C at 5°C / min, kept at that temperature for 4-4.5 hours, and then cooled to room temperature with the furnace.
6. The method for preparing the Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material according to claim 3, characterized in that: The polarization treatment in step (2) is as follows: first, the surface of the decarburized sintered product is polished; then, an electrode coating treatment is performed, i.e., silver electrodes are applied to the upper and lower surfaces of the decarburized sintered product after polishing; then, the temperature is raised to 700-800°C at 5°C / min for calcination, the temperature is kept for 20-30 minutes, and the product is cooled to room temperature with the furnace; finally, the product is polarized in high-temperature silicone oil at 180-200°C with a DC voltage of 10-15 kV / mm for a polarization time of 25-35 minutes.
7. A product obtained by the method for preparing Na / Sr / Ce / Cr / Ta / Mo doped CaBi2Nb2O9 high temperature piezoelectric ceramic material as claimed in any one of claims 3 to 6.
Citation Information
Patent Citations
Manganese-doped cerium lithium calcium titanoniobate-based ceramic material and preparation method thereof
CN105837200A
Calcium bismuth niobate high-temperature piezoceramic material of bismuth layer structure and preparing method of calcium bismuth niobate high-temperature piezoceramic material
CN106554203A
Nb-position Cr / Mo codoped bismuth-calcium niobate high-temperature piezoelectric ceramic material and preparation method therefor
CN109704761A
Ce, Cr and W co-doped CaBi4Ti4O15 high-temperature piezoelectric ceramic material and preparation method thereof
CN117263678A
Ce, Ga and Mo co-doped CaBi4Ti4O15 high-temperature piezoelectric ceramic material and preparation method thereof
CN117263679A
Cited By
Sr / Y / Ce / Cu / Ta / Zr / Mo doped Bi3TiNbO9 high-temperature piezoelectric ceramic material and preparation method thereof
CN119874359A
La / Nd / Ce / Ga / V / Sn / W doped Bi3TiNbO9 high-temperature piezoelectric ceramic material and preparation method thereof
CN119874360A
Y / La / Ce / Cr / Ta / Zr / W doped Bi3TiNbO9 high-temperature piezoelectric ceramic material and preparation method thereof
CN119874361A