Preparation method of aluminum nitride ceramic with high thermal conductivity

Through ball mill mixing and preheating reduction technology of AlN powder, Y2O3 powder and BN powder, combined with the use of BN crucibles and graphite molds, the problem of insufficient thermal conductivity and bending strength of aluminum nitride ceramics is solved, and high thermal conductivity and Preparation of aluminum nitride ceramics with high bending strength.

CN118908735AActive Publication Date: 2024-11-08FUJIAN HUAQING ELECTRONICS MATERIAL TECH

Patent Information

Application Number
CN202411207223.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The thermal conductivity and bending strength of aluminum nitride ceramics prepared in the prior art are relatively poor, and it is difficult to break through the thermal conductivity of 250W·m-1·K-1 and 500MPa.

Method used

Using ball mill mixing, preheating reduction and hot pressing sintering technology of AlN powder, Y2O3 powder and BN powder, preheating reduction and hot pressing sintering technology, the powder is mixed by ball mill to reduce the oxygen impurity content, and use BN crucibles and graphite molds during the sintering process to avoid Reaction and temperature control to form high density AlN ceramics.

Benefits of technology

Aluminum nitride ceramics with high thermal conductivity and high bending strength have a thermal conductivity of more than 250W·m-1·K-1, a bending strength of more than 500MPa, and improve the density and thermal conductivity of the ceramics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019362620000091
    Figure BDA0005019362620000091
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic preparation, provides a preparation method of aluminum nitride ceramic with high thermal conductivity, and solves the problem that the aluminum nitride ceramic prepared by the prior art is relatively poor in thermal conductivity and bending strength. Comprising the following preparation steps: 1) preparing raw materials; 2) ball-milling and mixing; 3) preheating reduction; and 4) hot pressed sintering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic preparation, and in particular to a method for preparing high thermal conductivity aluminum nitride ceramics. Background Art

[0002] Aluminum nitride (AlN) is a new generation of advanced heat dissipation material with high thermal conductivity (theoretically up to 320W·m -1 ·K -1 ), good insulation (>1014Ωcm), certain mechanical properties (bending strength 300-650MPa), thermal expansion coefficient equivalent to silicon, non-toxic, etc. It is often used as a substrate material, can resist the thermal stress shock caused by the circuit, and effectively dissipate heat.

[0003] Chinese patent application No. 202110920742.6 discloses an aluminum nitride ceramic tape-cast slurry, an aluminum nitride ceramic substrate and a preparation method. The aluminum nitride ceramic tape-cast slurry is made of the following raw materials in parts by mass: 100 parts of aluminum nitride powder, 3 to 10 parts of sintering aids, 1 to 6 parts of dispersants, 50 to 100 parts of organic solvents, 10 to 50 parts of binders, 1 to 15 parts of plasticizers and 0.5 to 2 parts of defoaming agents. The sintering aid is composed of component A and component B, component A is at least one of yttrium trioxide and calcium oxide, and component B is at least one of niobium pentoxide, cerium oxide and samarium oxide. Therefore, the sintering temperature of the aluminum nitride ceramic substrate does not exceed 1800°C, the sintering heating rate is higher than 5°C / min, and the sintering holding time can be less than 3 hours, which improves the efficiency of the preparation process without reducing the performance of the ceramic. However, the thermal conductivity of the aluminum nitride ceramics prepared by this invention is poor, only 175-184 W·m -1 ·K -1 .

[0004] Chinese patent application No. 202410606989.4 discloses an aluminum nitride ceramic sintered body and its preparation method and an aluminum nitride ceramic substrate, including aluminum nitride pure powder and a composite sintering aid, the composite sintering aid includes a Li-containing compound, a Ca-containing compound and a Y-containing compound, wherein the mass dosage relationship of each component in the composite sintering aid is: Y-containing compound>Ca-containing compound>Li-containing compound, wherein the mass of the Y-containing compound is calculated in the form of Y2O3, the mass of the Ca-containing compound is calculated in the form of CaF2, and the mass of the Li-containing compound is calculated in the form of Li2O. The aluminum nitride ceramic substrate of this invention has both high thermal conductivity and high flexural strength, wherein the thermal conductivity is 198-249W·m -1 ·K -1 , high bending strength greater than 500MPa. But the thermal conductivity still cannot exceed 250W·m -1 ·K -1 . Summary of the invention

[0005] Therefore, in view of the above problems, the present invention provides a method for preparing aluminum nitride ceramics with high thermal conductivity, which solves the problem that the thermal conductivity and bending strength of aluminum nitride ceramics prepared by the prior art are relatively poor.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing high thermal conductivity aluminum nitride ceramics comprises the following preparation steps:

[0008] S1. Preparation of raw materials: including AlN powder, Y2O3 powder, BN powder and anhydrous ethanol;

[0009] S2, ball milling and mixing: weigh 96-98 parts by weight of the AlN powder and 2-4 parts by weight of the Y2O3 powder, add them into a ball mill, mix them, and obtain a first mixed powder, add Al2O3 pellets at a mass ratio of the first mixed powder to Al2O3 pellets of 1:6-7, and then add anhydrous ethanol to the ball mill at a solid-liquid ratio of the first mixed powder to anhydrous ethanol of 1:1-1.5, introduce nitrogen protection, seal, and ball mill for 6-8 hours to obtain a slurry;

[0010] S3, preheating reduction: placing the slurry obtained in step S2 into a drying furnace to evaporate ethanol to obtain a second mixed powder, sieving the second mixed powder, and then adding it into a BN crucible, placing the BN crucible in a sintering furnace with a graphite generator at a pressure of 45-50 MPa, introducing nitrogen protection, raising the temperature to 1500-1550° C. at a heating rate of 100° C. / min, keeping the temperature for 1-4 hours, and then cooling it to room temperature at a cooling rate of 10° C. / min to obtain a third mixed powder;

[0011] S4, hot pressing sintering: transferring the third mixed powder preheated and reduced in step S3 to a hot pressing mold, placing the hot pressing mold in a vacuum hot pressing sintering furnace for hot pressing sintering at a pressure of 30-35 MPa, raising the temperature to 1750-1800°C at a heating rate of 10°C / min, keeping the temperature for 5-6 hours, and then cooling to room temperature at a cooling rate of 5°C / min to obtain the high thermal conductivity aluminum nitride ceramic;

[0012] The hot pressing mold is made of graphite, and a BN powder coating is provided inside the hot pressing mold; the BN crucible includes a crucible body and a crucible cover, and the crucible cover is provided with array holes.

[0013] Furthermore, the preparation process of the BN powder is as follows:

[0014] a. Boric acid and melamine are mixed in a molar ratio of 2-3:1 to obtain a mixture, and the mixture is dispersed in deionized water in a solid-liquid ratio of 1:20-25 to deionized water, heated in a water bath at 95-100° C., stirred until completely dissolved, then the temperature is reduced to 80-85° C. and kept warm for 6-8 hours, and cooled to room temperature to obtain a mixed solution;

[0015] b. Filtering the mixed solution obtained in step a, taking the filter cake and drying it to obtain a boron nitride precursor;

[0016] c. Transfer the boron nitride precursor obtained in step b to a tubular furnace, introduce nitrogen protection, raise the temperature to 1000-1050° C., keep warm for 4-6 hours, and cool to room temperature to obtain the BN powder.

[0017] Furthermore, the particle size of the BN powder is 50-500 nm.

[0018] Furthermore, the particle size of the Al2O3 spherical particles is 20-100 nm.

[0019] Furthermore, the oxygen content of the AlN powder is 0.85 wt %.

[0020] Furthermore, the purity of the Y2O3 is ≥ 99.99%

[0021] Furthermore, the nitrogen protection is: nitrogen is introduced at a flow rate of 2 L / min, and the purity of the nitrogen is ≧99.999%.

[0022] By adopting the above technical solution, the beneficial effects of the present invention are:

[0023] 1. The key to obtain high thermal conductivity AlN ceramics is to avoid the influence of oxygen impurities and prevent excessive oxygen from entering the AlN lattice. Pre-reduction can effectively reduce the oxygen content of the powder and reduce the introduction of oxygen elements. In addition, during the sintering process, Al2O3 reacts with Y2O3 to co-generate Al5Y3O 12 , YAlO and Y4Al2O9 three crystal edge phases. After the AlN grains weaken the powder oxide layer, the grain edge phase changes from YAlO to Y4Al2O9. Y4Al2O9 is more conducive to purifying oxygen impurities in the AlN lattice and realizing the high thermal conductivity of AlN ceramics, so that the prepared AlN ceramics have both high thermal conductivity and high bending strength.

[0024] 2. Higher density of AlN ceramics can withstand greater external forces and improve its bending strength and hardness. Sintering at a lower temperature can improve the density of AlN ceramics, the holes between AlN grains become smaller, the generation of pores is reduced, and the area of ​​crystal edge phase flow and convergence can be smaller, thereby producing a more uniform and fine grain edge phase.

[0025] 3. In the preheating and reduction step, the sieved second mixed powder is added to a BN crucible, and then the BN crucible is placed in a sintering furnace with a graphite generator for preheating and reduction. Ordinary graphite crucibles are not used because BN crucibles are chemically inert to most molten metals, glass and slag, and can effectively prevent the crucible from reacting with molten metal Al2O3 and affecting the thermal conductivity of AlN ceramics; secondly, the thermal conductivity of the BN crucible does not change with temperature, which is particularly important for the AlN ceramic production process that requires accurate temperature control, so as to avoid the heating process from affecting the temperature of preheating and reduction; similarly, a BN powder coating is provided inside the hot pressing mold to prevent the crucible from reacting with molten metal Al2O3 and to accurately control the temperature of the sintering reaction. DETAILED DESCRIPTION

[0026] Example 1

[0027] A method for preparing high thermal conductivity aluminum nitride ceramics comprises the following preparation steps:

[0028] (1) Preparation of raw materials: including AlN powder with an oxygen content of 0.85 wt%, Y2O3 powder with a purity of ≥99.99%, BN powder with a particle size of 180 nm, and anhydrous ethanol;

[0029] (2) Preparation of BN powder

[0030] (2-1) Boric acid and melamine are mixed in a molar ratio of 2:1 to obtain a mixture, the mixture is dispersed in deionized water in a solid-liquid ratio of 1:20 to deionized water, heated in a water bath at 95° C., stirred until completely dissolved, then the temperature is reduced to 80° C. and kept for 6 hours, and cooled to room temperature to obtain a mixed solution;

[0031] (2-2) filtering the mixed solution obtained in step a, taking the filter cake and drying it to obtain a boron nitride precursor;

[0032] (2-3) transferring the boron nitride precursor obtained in step b into a tube furnace, introducing nitrogen protection, raising the temperature to 1050° C., keeping the temperature for 4 hours, and cooling to room temperature to obtain the BN powder;

[0033] (3) Ball milling and mixing: Weigh 98 parts by weight of the AlN powder and 2 parts by weight of the Y2O3 powder, add them into a ball mill, mix them, and obtain a first mixed powder. Al2O3 pellets are added in a mass ratio of 1:6 between the first mixed powder and the Al2O3 pellets, and the particle size of the Al2O3 pellets is 20 nm. Anhydrous ethanol is added into the ball mill in a solid-liquid ratio of 1:1 between the first mixed powder and anhydrous ethanol. Nitrogen with a purity of ≧99.999% is introduced at a flow rate of 2 L / min for protection. The mixture is sealed and ball milled for 6 h to obtain a slurry.

[0034] (4) Preheating reduction: placing the slurry obtained in step (3) into a drying furnace to evaporate ethanol to obtain a second mixed powder, sieving the second mixed powder, and then adding it into a BN crucible, wherein the BN crucible comprises a crucible body and a crucible cover, and the crucible cover is provided with an array of holes, placing the BN crucible in a sintering furnace with a graphite generator at a pressure of 45 MPa, introducing nitrogen with a purity of ≧99.999% at a flow rate of 2 L / min for protection, raising the temperature to 1550° C. at a heating rate of 100° C. / min, keeping the temperature for 2 h, and then cooling to room temperature at a cooling rate of 10° C. / min to obtain a third mixed powder;

[0035] (5) Hot pressing sintering: The third mixed powder preheated and reduced in step (4) is transferred to a hot pressing mold made of graphite, wherein a BN powder coating is provided inside the hot pressing mold. The hot pressing mold is placed in a vacuum hot pressing sintering furnace for hot pressing sintering at a pressure of 35 MPa. The temperature is increased to 1750°C at a heating rate of 10°C / min, maintained for 5 hours, and then cooled to room temperature at a cooling rate of 5°C / min to obtain the high thermal conductivity aluminum nitride ceramic.

[0036] Example 2

[0037] A method for preparing high thermal conductivity aluminum nitride ceramics comprises the following preparation steps:

[0038] (1) Preparation of raw materials: including AlN powder with an oxygen content of 0.85 wt%, Y2O3 powder with a purity of ≥99.99%, BN powder with a particle size of 200 nm, and anhydrous ethanol;

[0039] (2) Preparation of BN powder

[0040] (2-1) mixing boric acid and melamine in a molar ratio of 2:1 to obtain a mixture, dispersing the mixture in deionized water in a solid-liquid ratio of 1:20 to deionized water, heating in a water bath at 100° C., stirring until completely dissolved, then reducing the temperature to 80° C. and maintaining the temperature for 8 h, and cooling to room temperature to obtain a mixed solution;

[0041] (2-2) filtering the mixed solution obtained in step a, taking the filter cake and drying it to obtain a boron nitride precursor;

[0042] (2-3) transferring the boron nitride precursor obtained in step b into a tube furnace, introducing nitrogen protection, raising the temperature to 1050° C., keeping the temperature for 4 hours, and cooling to room temperature to obtain the BN powder;

[0043] (3) Ball milling and mixing: 96 parts by weight of the AlN powder and 4 parts by weight of the Y2O3 powder were weighed and added to a ball mill, mixed to obtain a first mixed powder, Al2O3 pellets were added at a mass ratio of 1:6.5 between the first mixed powder and Al2O3 pellets, and the particle size of the Al2O3 pellets was 50 nm, and then anhydrous ethanol was added to the ball mill at a solid-liquid ratio of 1:1.5 between the first mixed powder and anhydrous ethanol, and nitrogen with a purity of ≧99.999% was introduced at a flow rate of 2 L / min for protection, the mixture was sealed, and ball milling was performed for 8 h to obtain a slurry;

[0044] (4) Preheating reduction: placing the slurry obtained in step (3) into a drying furnace to evaporate ethanol to obtain a second mixed powder, sieving the second mixed powder, and then adding it into a BN crucible, wherein the BN crucible comprises a crucible body and a crucible cover, and the crucible cover is provided with an array of holes, placing the BN crucible in a sintering furnace with a graphite generator at a pressure of 45 MPa, introducing nitrogen with a purity of ≧99.999% at a flow rate of 2 L / min for protection, raising the temperature to 1550° C. at a heating rate of 100° C. / min, keeping the temperature for 3 h, and then cooling to room temperature at a cooling rate of 10° C. / min to obtain a third mixed powder;

[0045] (5) Hot pressing sintering: The third mixed powder preheated and reduced in step (4) is transferred to a hot pressing mold made of graphite, wherein a BN powder coating is provided inside the hot pressing mold. The hot pressing mold is placed in a vacuum hot pressing sintering furnace for hot pressing sintering at a pressure of 30 MPa. The temperature is increased to 1780°C at a heating rate of 10°C / min, maintained for 5 hours, and then cooled to room temperature at a cooling rate of 5°C / min to obtain the high thermal conductivity aluminum nitride ceramic.

[0046] Example 3

[0047] A method for preparing high thermal conductivity aluminum nitride ceramics comprises the following preparation steps:

[0048] (1) Preparation of raw materials: including AlN powder with an oxygen content of 0.85 wt%, Y2O3 powder with a purity of ≥99.99%, BN powder with a particle size of 200 nm, and anhydrous ethanol;

[0049] (2) Preparation of BN powder

[0050] (2-1) Boric acid and melamine are mixed in a molar ratio of 2:1 to obtain a mixture, the mixture is dispersed in deionized water in a solid-liquid ratio of 1:25 to deionized water, heated in a water bath at 100° C., stirred until completely dissolved, then the temperature is reduced to 85° C. and kept warm for 7 h, and cooled to room temperature to obtain a mixed solution;

[0051] (2-2) filtering the mixed solution obtained in step a, taking the filter cake and drying it to obtain a boron nitride precursor;

[0052] (2-3) transferring the boron nitride precursor obtained in step b into a tube furnace, introducing nitrogen protection, raising the temperature to 1050° C., keeping the temperature for 5 hours, and cooling to room temperature to obtain the BN powder;

[0053] (3) Ball milling and mixing: 97 parts by weight of the AlN powder and 3 parts by weight of the Y2O3 powder were weighed and added to a ball mill, and mixed to obtain a first mixed powder. Al2O3 pellets were added at a mass ratio of 1:7 between the first mixed powder and the Al2O3 pellets, and the particle size of the Al2O3 pellets was 100 nm. Anhydrous ethanol was then added to the ball mill at a solid-liquid ratio of 1:1 between the first mixed powder and anhydrous ethanol. Nitrogen with a purity of ≧99.999% was introduced at a flow rate of 2 L / min for protection. The mixture was sealed and ball milled for 7 h to obtain a slurry.

[0054] (4) Preheating reduction: placing the slurry obtained in step (3) into a drying furnace to evaporate ethanol to obtain a second mixed powder, sieving the second mixed powder, and then adding it into a BN crucible, wherein the BN crucible comprises a crucible body and a crucible cover, and the crucible cover is provided with an array of holes, placing the BN crucible in a sintering furnace with a graphite generator at a pressure of 50 MPa, introducing nitrogen with a purity of ≧99.999% at a flow rate of 2 L / min for protection, raising the temperature to 1550° C. at a heating rate of 100° C. / min, keeping the temperature for 4 h, and then cooling to room temperature at a cooling rate of 10° C. / min to obtain a third mixed powder;

[0055] (5) Hot pressing sintering: The third mixed powder preheated and reduced in step (4) is transferred to a hot pressing mold made of graphite, wherein a BN powder coating is provided inside the hot pressing mold. The hot pressing mold is placed in a vacuum hot pressing sintering furnace for hot pressing sintering at a pressure of 35 MPa. The temperature is increased to 1800° C. at a heating rate of 10° C. / min, maintained for 5 h, and then cooled to room temperature at a cooling rate of 5° C. / min to obtain the high thermal conductivity aluminum nitride ceramic.

[0056] Comparative Example 1

[0057] The difference from Example 1 is that the raw materials do not use the AlN powder, Y2O3 powder, BN powder and anhydrous ethanol in the present invention. The raw materials used include: 100 parts of aluminum nitride powder, 3 parts of sintering aids, 1 part of dispersant, 50 parts of organic solvents, 10 parts of binders, 1 part of plasticizers, and 0.5 parts of degassing agents. The sintering aids include Y2O3 and niobium pentoxide, and the ratio of Y2O3 to niobium pentoxide is 1:2. The dispersant is triolein, the organic solvent is isopropanol, the binder is polyvinyl butyral, the plasticizer is dibutyl phthalate, and the degassing agent is octanol. The preparation steps do not include the preparation of BN powder and preheating reduction. The preparation steps include: ball milling and mixing of the raw materials, casting and slicing to prepare a cast sheet, punching, debinding and sintering to obtain an aluminum nitride ceramic product. Other technical solutions are the same as Example 1.

[0058] Comparative Example 2

[0059] The difference from Example 1 is that the raw materials do not use the AlN powder, Y2O3 powder, BN powder and anhydrous ethanol in the present invention. The raw materials used include: 100 parts of aluminum nitride powder, 5 parts of sintering aids, 3 parts of dispersants, 80 parts of organic solvents, 30 parts of binders, 10 parts of plasticizers, and 1 part of degassing agent. The sintering aids include Y2O3 and niobium pentoxide, and the ratio of Y2O3 to niobium pentoxide is 1:2. The dispersant is triolein, the organic solvent is isopropanol, the binder is polyvinyl butyral, the plasticizer is dibutyl phthalate, and the degassing agent is octanol. The preparation steps do not include the preparation of BN powder and preheating reduction. The preparation steps include: ball milling and mixing of the raw materials, casting and slicing to prepare a cast sheet, punching, debinding and sintering to obtain an aluminum nitride ceramic product. Other technical solutions are the same as Example 1.

[0060] Comparative Example 3

[0061] The difference from Example 1 is that the raw materials do not use the AlN powder, Y2O3 powder, BN powder and anhydrous ethanol in the present invention, and the raw materials used include: 100 parts of aluminum nitride powder, 10 parts of sintering aids, 6 parts of dispersants, 100 parts of organic solvents, 50 parts of binders, 15 parts of plasticizers, and 2 parts of degassing agents. The sintering aids include Y2O3 and niobium pentoxide, and the ratio of Y2O3 to niobium pentoxide is 1:2. The dispersant is triolein, the organic solvent is isopropanol, the binder is polyvinyl butyral, the plasticizer is dibutyl phthalate, and the degassing agent is octanol. The preparation steps do not include the preparation of BN powder and preheating reduction. The preparation steps include: ball milling and mixing of the raw materials, casting and slicing to prepare a cast sheet, punching, debinding and sintering to obtain an aluminum nitride ceramic product. Other technical solutions are the same as Example 1.

[0062] The performance test results of the products of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, Comparative Example 3 are shown in the following table.

[0063] Table 1

[0064]

[0065] The thermal conductivity, bending strength and density of the products of Example 1, Example 2 and Example 3 all show good results, which indicates that the aluminum nitride ceramics prepared by the present invention have good quality.

[0066] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.

Claims

1. A method for preparing high thermal conductivity aluminum nitride ceramics, It is characterized in that The method comprises the following preparation steps: S1. Preparation of raw materials: including AlN powder, Y 2 O 3 powder, BN powder and anhydrous ethanol; S2, ball milling and mixing: weigh 96-98 parts by weight of the AlN powder and 2-4 parts by weight of Y 2 O 3 The powder is added into a ball mill and mixed to obtain a first mixed powder. 2 O 3 The mass ratio of the pellets is 1:6-7, and Al is added 2 O 3 Then, according to the solid-liquid ratio of the first mixed powder to anhydrous ethanol of 1:1-1.5, anhydrous ethanol is added into a ball mill, nitrogen is introduced for protection, the mixture is sealed, and ball milling is performed for 6-8 hours to obtain a slurry; S3, preheating reduction: placing the slurry obtained in step S2 into a drying furnace to evaporate ethanol to obtain a second mixed powder, sieving the second mixed powder, and then adding it into a BN crucible, placing the BN crucible in a sintering furnace with a graphite generator at a pressure of 45-50 MPa, introducing nitrogen protection, raising the temperature to 1500-1550° C. at a heating rate of 100° C. / min, keeping the temperature for 1-4 hours, and then cooling it to room temperature at a cooling rate of 10° C. / min to obtain a third mixed powder; S4, hot pressing sintering: transferring the third mixed powder preheated and reduced in step S3 to a hot pressing mold, placing the hot pressing mold in a vacuum hot pressing sintering furnace for hot pressing sintering at a pressure of 30-35 MPa, raising the temperature to 1750-1800°C at a heating rate of 10°C / min, keeping the temperature for 5-6 hours, and then cooling to room temperature at a cooling rate of 5°C / min to obtain the high thermal conductivity aluminum nitride ceramic; The hot pressing mold is made of graphite, and a BN powder coating is provided inside the hot pressing mold; the BN crucible includes a crucible body and a crucible cover, and the crucible cover is provided with array holes.

2. A method for preparing a high thermal conductivity aluminum nitride ceramic according to claim 1, It is characterized in that The preparation process of the BN powder is as follows: a. Boric acid and melamine are mixed in a molar ratio of 2-3:1 to obtain a mixture, and the mixture is dispersed in deionized water in a solid-liquid ratio of 1:20-25 to deionized water, heated in a water bath at 95-100° C., stirred until completely dissolved, then the temperature is reduced to 80-85° C. and kept warm for 6-8 hours, and cooled to room temperature to obtain a mixed solution; b. Filtering the mixed solution obtained in step a, taking the filter cake and drying it to obtain a boron nitride precursor; c. Transfer the boron nitride precursor obtained in step b to a tubular furnace, introduce nitrogen protection, raise the temperature to 1000-1050° C., keep warm for 4-6 hours, and cool to room temperature to obtain the BN powder.

3. The method for preparing a high thermal conductivity aluminum nitride ceramic according to claim 1, Features: The particle size of the BN powder is 50-500 nm.

4. The method for preparing a high thermal conductivity aluminum nitride ceramic according to claim 1, Features: The Al 2 O 3 The particle size of the spherules is 20-100 nm.

5. The method for preparing a high thermal conductivity aluminum nitride ceramic according to claim 1, Features: The oxygen content of the AlN powder is 0.85 wt %.

6. The method for preparing a high thermal conductivity aluminum nitride ceramic according to claim 1, Features: The Y 2 O 3 The purity is ≧99.99%.

7. A method for preparing a high thermal conductivity aluminum nitride ceramic according to any one of claims 1-2, It is characterized in that The nitrogen protection is as follows: nitrogen is introduced at a flow rate of 2 L / min, and the purity of the nitrogen is ≧99.999%.

Citation Information

Patent Citations

  • Method for making high-thermal-conductivity aluminium nitride ceramics substrate

    CN101333114A

  • Method for preparing high-strength and high-thermal-conductivity aluminum nitride through hot pressed sintering

    CN112811909A

  • BN nanosheet toughened high-thermal-conductivity AlN ceramic substrate and preparation method thereof

    CN113213944A

  • Aluminum nitride ceramic sintered body, preparation method thereof and aluminum nitride ceramic substrate

    CN118164766A

  • Slurry and preparation method for high-performance aluminum nitride ceramic substrate

    WO2022100249A1

Cited By

  • Preparation method of high-heat-conductivity aluminum nitride substrate

    CN121673062A

  • A method for preparing a high-thermal-conductivity aluminum nitride substrate

    CN121673062B