Graphite boat saturated film layer structure and preparation method thereof
By forming a saturated film layer structure composed of adhesive, compound nano powder, functional filler, functional additive and sintering agent on the graphite boat, the shortcomings of graphite boat in corrosion resistance and reducing product defect rate are solved. , achieving more efficient silicon wafer coating uniformity and quality assurance.
Patent Information
- Application Number
- CN202410995080.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing graphite boat saturated film structure has shortcomings in corrosion resistance and reducing product defect rate, making it difficult to effectively ensure the uniformity and quality of silicon wafer coating.
Using a saturated film structure composed of adhesive, compound nano powder, functional filler, functional additive and sintering agent, through multiple hot pressing and sintering treatments at different temperatures, a densified composite ceramic coating is formed to enhance the The corrosion resistance and coating uniformity of graphite boats.
It realizes excellent corrosion resistance and reduces product defect rate of the graphite boat saturated film structure, ensures uniformity and quality of the coating, and is suitable for the production of solar silicon wafers.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of graphite boat production, in particular to a graphite boat saturated film layer structure and a preparation method thereof. Background Art
[0002] Graphite boat is a graphite mold. The graphite mold itself is a carrier. The raw materials and parts that need to be positioned or shaped can be placed in the graphite mold together and sintered at high temperature. The graphite mold is made of artificial graphite through mechanical processing and has corresponding electrode sheets. The electrode sheets serve as the positive and negative poles of the power supply, thereby generating an electric field, ionizing the gas into plasma, and forming a new film layer.
[0003] There is a process called PECVD coating in the production and processing of solar silicon wafers, which is used to improve the solar energy conversion rate of silicon wafers. The PECVD coating process requires the use of a graphite boat. The specific method is to put the silicon wafer to be coated in the graphite boat, and a chemical reaction will occur under certain conditions to coat a layer of film on the surface of the silicon wafer.
[0004] In the patent document with application number "CN202311862265.8" and titled "A graphite evaporation boat and its preparation method", it is recorded that "a coating structure is formed on the evaporation side of the evaporation boat, and the coating structure includes the following components in mass fraction: matrix filler 60%-80%; silicon 10-15%; nickel-aluminum composite powder, 1-5%; thermal conductive filler, 10-15%; adhesive 0.5-2%; the coating structure is formed by hot pressing and sintering at increasing temperatures in batches. The present invention is based on a multi-component coating, and the components are easily diffused by melts of different components through multiple hot pressing and sintering treatments at different temperatures. The internal crystalline components undergo multi-phase melting and reaction during the sintering process to gradually form a densified composite ceramic coating, which can improve the corrosion resistance of the graphite evaporation boat." Although this patent can achieve the effect of corrosion resistance, it is relatively insufficient in reducing the product defective rate when used, and still needs further improvement.
[0005] For example, the patent document with application number "CN202121290943.4" and name "Graphite boat saturated film layer structure and graphite boat for PERC solar cells" records that "it includes a first film layer, a second film layer and a third film layer deposited in sequence on the surface of the graphite boat body, the first film layer is a silicon carbide film or a silicon nitride film, the second film layer is an aluminum oxide film, and the third film layer is a silicon carbide film or a silicon nitride film. The saturated film layer structure of the graphite boat provided by the utility model can make the electric field distribution on the surface of the graphite boat more uniform, and make the saturated film layer structure of the graphite boat more stable, so as to make the silicon wafer coating uniformity better and prevent the problem of partial dark films and black edges on the coated silicon wafers." Although this patent can be used in the production of solar cells, its corrosion resistance and other properties are relatively insufficient and still need further improvement.
[0006] Based on this, the present invention provides a graphite boat saturated film layer structure and a preparation method thereof to solve the above-mentioned technical problems! Summary of the invention
[0007] The object of the present invention is to provide a graphite boat saturated film layer structure and a preparation method thereof. The prepared graphite boat saturated film layer structure not only has excellent corrosion resistance, but also has the effect of reducing product defective rate when used, effectively ensuring its quality.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] The first aspect of the present invention provides a graphite boat saturated film layer structure, comprising a graphite boat body and a saturated film layer arranged on the surface of the graphite boat body;
[0010] The saturated film layer is composed of the following raw materials in parts by weight: 20 to 30 parts of adhesive, 3 to 6 parts of compound nano powder, 3 to 5 parts of functional filler, 2 to 4 parts of functional additive and 4 to 7 parts of sintering aid.
[0011] Furthermore, the adhesive is selected from any one of epoxy resin adhesive and acrylic adhesive.
[0012] Furthermore, the compound nano powder is formed by mixing silicon, molybdenum and chromium in a mass ratio of 1:0.12-0.22:0.08-0.13.
[0013] Furthermore, the functional filler is formed by mixing and compounding the modified filler and alumina in a mass ratio of 1:0.08 to 0.28.
[0014] Furthermore, the preparation process of the modified filler is as follows:
[0015] Place an appropriate amount of carbon nitride powder in an appropriate amount of modified liquid at a solid-liquid ratio of 0.01-0.12 g / mL, stir at 30-50 r / min for 10-14 min, then ultrasonically treat for 20-30 min, then treat at a water bath temperature of 25-30 min and 120-140 r / min for 100-120 min, and after suction filtration, wash the filter cake with anhydrous ethanol and deionized water for 2-4 times respectively;
[0016] After washing, the filler is placed in a vacuum drying device at 60-70°C and dried for 12-14 hours to obtain a modified filler.
[0017] Furthermore, the modified liquid is prepared by mixing the composite material and distilled water in a mass ratio of 0.12 to 0.22:1.
[0018] Furthermore, the composite material is formed by mixing aluminum phosphate and sodium phosphate in a mass ratio of 1:0.2 to 0.4.
[0019] Furthermore, the preparation process of the functional additive is as follows:
[0020] Aluminum nitride, oxalic acid and nickel acetate tetrahydrate are placed in a stirring device and mixed thoroughly in a mass ratio of 1:0.26-0.36:0.12-0.24, and then placed in a grinding device and ground for 20-30 minutes to obtain a grinding product;
[0021] The obtained ground product is placed in a nitrogen atmosphere and subjected to a two-stage high temperature treatment to obtain a functional additive;
[0022] Among them, the two-stage high temperature process is as follows:
[0023] The first stage: heating to 420℃ at a heating rate of 4-5℃ / min, and heat preservation for 20-30min;
[0024] The second stage: heating to 500°C at a heating rate of 8°C / min and keeping warm for 40 to 50 minutes.
[0025] Furthermore, the sintering aid is formed by mixing nano magnesium oxide and nano zirconium dioxide in a mass ratio of 1:0.06 to 0.12.
[0026] The second aspect of the present invention: also provides a method for preparing the above-mentioned graphite boat saturated film layer structure, characterized in that it comprises the following steps:
[0027] Step 1: accurately weigh the adhesive, compound nano powder, functional filler, functional additive and sintering agent, and put the adhesive, compound nano powder, functional filler, functional additive and sintering agent into a mixing device for mixing and stirring to obtain a film material;
[0028] Step 2: coating the obtained film material on the surface of the cleaned graphite boat body, then heating to 105-120° C. and keeping the temperature for 5-8 minutes;
[0029] Step 3: In a vacuum environment of 6-12 Pa, the temperature is raised to 720-740° C. at a heating rate of 120-140° C. / min, and the temperature is kept for 6-10 minutes;
[0030] Step 4: Heat the temperature to 1720-1740°C at a heating rate of 80-100°C / min using nitrogen, and keep the temperature and pressure for 120-140 minutes under a hot pressing pressure of 28-30 MPa. After cooling, the product can be inspected.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The saturated film layer structure of a graphite boat provided by the present invention comprises a graphite boat body and a saturated film layer arranged on the surface of the graphite boat body, wherein the saturated film layer uses adhesive, compounded nano powder, functional filler, functional auxiliary agent and sintering aid as raw materials, wherein the compounded nano powder is compounded by mixing silicon, molybdenum and chromium, the functional filler is compounded by mixing modified filler and alumina, the functional auxiliary agent is obtained by mixing and grinding aluminum nitride, oxalic acid and nickel acetate tetrahydrate, and then subjecting them to high temperature treatment in a nitrogen atmosphere using a two-stage high temperature method, and the sintering aid is obtained by mixing nano magnesium oxide and nano zirconium dioxide; the saturated film layer structure of a graphite boat provided by the present invention is obtained by putting adhesive, compounded nano powder, functional filler, functional auxiliary agent and sintering aid into a mixing device for mixing and stirring to obtain a film material, and then coating the obtained film material on the surface of the cleaned graphite boat body, and then sintering, cooling, and then undergoing an inspection process. The graphite boat saturated film layer structure prepared by the present invention not only has excellent corrosion resistance, but also has the effect of reducing the product defect rate when used, effectively ensuring its quality. The graphite boat saturated film layer structure and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] This embodiment provides a graphite boat saturated film layer structure, including a graphite boat body and a saturated film layer arranged on the surface of the graphite boat body;
[0036] The saturated film layer is composed of the following raw materials in parts by weight: 20 parts of adhesive, 3 parts of compound nano powder, 3 parts of functional filler, 2 parts of functional additive and 4 parts of sintering aid.
[0037] Among them, the adhesive is epoxy resin adhesive.
[0038] In this embodiment, it should be noted that the epoxy resin adhesive was purchased from Shandong Huachen New Materials Co., Ltd.
[0039] The compound nano powder is prepared by mixing silicon, molybdenum and chromium in a mass ratio of 1:0.12:0.08.
[0040] Furthermore, the functional filler is compounded by mixing the modified filler and alumina in a mass ratio of 1:0.08.
[0041] The preparation process of the modified filler is as follows:
[0042] An appropriate amount of carbon nitride powder was placed in an appropriate amount of modified liquid at a solid-liquid ratio of 0.01 g / mL, stirred at 30 r / min for 10 min, then ultrasonically treated for 20 min, and then treated at a water bath temperature of 25 min and 120 r / min for 100 min. After suction filtration, the filter cake was washed twice with anhydrous ethanol and deionized water respectively;
[0043] After washing, the mixture was placed in a vacuum drying device at 60°C and dried for 12 hours to obtain a modified filler.
[0044] In addition, the modified liquid is mixed with the composite material and distilled water in a mass ratio of 0.12:1.
[0045] The composite material is prepared by mixing aluminum phosphate and sodium phosphate in a mass ratio of 1:0.2.
[0046] The preparation process of functional additives is as follows:
[0047] Aluminum nitride, oxalic acid and nickel acetate tetrahydrate were placed in a stirring device and mixed thoroughly in a mass ratio of 1:0.26:0.12, and then placed in a grinding device and ground for 20 minutes to obtain a grinding product;
[0048] The obtained ground product is placed in a nitrogen atmosphere and subjected to a two-stage high temperature treatment to obtain a functional additive;
[0049] Among them, the two-stage high temperature process is as follows:
[0050] The first stage: heating to 420℃ at a heating rate of 4℃ / min and keeping the temperature for 20min;
[0051] The second stage: heating to 500°C at a heating rate of 8°C / min and keeping the temperature for 40 minutes.
[0052] Furthermore, the sintering aid is a mixture of nano magnesium oxide and nano zirconium dioxide in a mass ratio of 1:0.06.
[0053] In addition, this embodiment also provides a method for preparing the above-mentioned graphite boat saturated film layer structure, which is characterized by comprising the following steps:
[0054] Step 1: accurately weigh the adhesive, compound nano powder, functional filler, functional additive and sintering agent, and put the adhesive, compound nano powder, functional filler, functional additive and sintering agent into a mixing device for mixing and stirring to obtain a film material;
[0055] Step 2: coating the obtained film material on the surface of the cleaned graphite boat body, then heating to 105° C. and keeping the temperature for 5 minutes;
[0056] The coating thickness is 0.8 mm.
[0057] Step 3: In a vacuum environment of 6 Pa, the temperature is increased to 720°C at a heating rate of 120°C / min, and the temperature is kept for 6 minutes;
[0058] Step 4: Heat the temperature to 1720°C at a heating rate of 80°C / min using nitrogen, and keep the temperature and pressure for 120 minutes under a hot pressing pressure of 28 MPa. After cooling, the product can be inspected.
[0059] Example 2
[0060] The preparation method of the graphite boat saturated film structure provided in this embodiment is basically the same as that in embodiment 1, except that: the specific raw material composition and the specific preparation method of the graphite boat saturated film structure in this embodiment are different; the specific raw material composition and the specific preparation method of the graphite boat saturated film structure in this embodiment are as follows:
[0061] This embodiment provides a graphite boat saturated film layer structure, including a graphite boat body and a saturated film layer arranged on the surface of the graphite boat body;
[0062] The saturated film layer is composed of the following raw materials in parts by weight: 25 parts of adhesive, 4 parts of compound nano powder, 4 parts of functional filler, 3 parts of functional additive and 5 parts of sintering aid.
[0063] Among them, the adhesive is acrylic adhesive.
[0064] In this embodiment, it should be noted that the acrylic adhesive was purchased from Shantou Yulong New Material Technology Co., Ltd.
[0065] The compound nano powder is prepared by mixing silicon, molybdenum and chromium in a mass ratio of 1:0.17:0.11.
[0066] Furthermore, the functional filler is compounded by mixing the modified filler and alumina in a mass ratio of 1:0.18.
[0067] The preparation process of the modified filler is as follows:
[0068] An appropriate amount of carbon nitride powder was placed in an appropriate amount of modified liquid at a solid-liquid ratio of 0.07 g / mL, stirred at 340 r / min for 12 min, then ultrasonically treated for 25 min, and then treated at a water bath temperature of 27 min and 130 r / min for 110 min. After suction filtration, the filter cake was washed three times with anhydrous ethanol and deionized water respectively;
[0069] After washing, the mixture was placed in a vacuum drying device at 65°C and dried for 13 hours to obtain a modified filler.
[0070] In addition, the modified liquid is mixed with the composite material and distilled water in a mass ratio of 0.17:1.
[0071] The composite material is made by mixing aluminum phosphate and sodium phosphate in a mass ratio of 1:0.3.
[0072] The preparation process of functional additives is as follows:
[0073] Aluminum nitride, oxalic acid and nickel acetate tetrahydrate were placed in a stirring device and mixed thoroughly in a mass ratio of 1:0.31:0.18, and then placed in a grinding device and ground for 25 minutes to obtain a grinding product;
[0074] The obtained ground product is placed in a nitrogen atmosphere and subjected to a two-stage high temperature treatment to obtain a functional additive;
[0075] Among them, the two-stage high temperature process is as follows:
[0076] The first stage: heating to 420℃ at a heating rate of 5℃ / min and keeping the temperature for 25min;
[0077] The second stage: heating to 500°C at a heating rate of 8°C / min and keeping the temperature for 45 minutes.
[0078] Furthermore, the sintering aid is a mixture of nano magnesium oxide and nano zirconium dioxide in a mass ratio of 1:0.09.
[0079] In addition, this embodiment also provides a method for preparing the above-mentioned graphite boat saturated film layer structure, which is characterized by comprising the following steps:
[0080] Step 1: accurately weigh the adhesive, compound nano powder, functional filler, functional additive and sintering agent, and put the adhesive, compound nano powder, functional filler, functional additive and sintering agent into a mixing device for mixing and stirring to obtain a film material;
[0081] Step 2: coating the obtained film material on the surface of the cleaned graphite boat body, then heating to 115° C. and keeping the temperature for 6 minutes;
[0082] The coating thickness is 0.8 mm.
[0083] Step 3: In a vacuum environment of 8 Pa, the temperature is increased to 730° C. at a heating rate of 130° C. / min, and the temperature is kept for 8 minutes;
[0084] Step 4: Heat the temperature to 1730°C at a heating rate of 90°C / min using nitrogen, and keep the temperature and pressure for 130 minutes under a hot pressing pressure of 29 MPa. After cooling, the product can be inspected.
[0085] Example 3
[0086] The preparation method of the graphite boat saturated film structure provided in this embodiment is basically the same as that in embodiment 1, except that: the specific raw material composition and the specific preparation method of the graphite boat saturated film structure in this embodiment are different; the specific raw material composition and the specific preparation method of the graphite boat saturated film structure in this embodiment are as follows:
[0087] This embodiment provides a graphite boat saturated film layer structure, including a graphite boat body and a saturated film layer arranged on the surface of the graphite boat body;
[0088] The saturated film layer is composed of the following raw materials in parts by weight: 30 parts of adhesive, 6 parts of compound nano powder, 5 parts of functional filler, 4 parts of functional additive and 7 parts of sintering aid.
[0089] Among them, the adhesive is epoxy resin adhesive.
[0090] In this embodiment, it should be noted that the epoxy resin adhesive was purchased from Shandong Huachen New Materials Co., Ltd.
[0091] The compound nano powder is prepared by mixing silicon, molybdenum and chromium in a mass ratio of 1:0.22:0.13.
[0092] Furthermore, the functional filler is compounded by mixing the modified filler and alumina in a mass ratio of 1:0.28.
[0093] The preparation process of the modified filler is as follows:
[0094] An appropriate amount of carbon nitride powder was placed in an appropriate amount of modified liquid at a solid-liquid ratio of 0.12 g / mL, stirred at 50 r / min for 14 min, then ultrasonically treated for 30 min, and then treated at a water bath temperature of 30 min and 140 r / min for 120 min. After suction filtration, the filter cake was washed 4 times with anhydrous ethanol and deionized water respectively;
[0095] After washing, the mixture was placed in a vacuum drying device at 70°C and dried for 14 hours to obtain a modified filler.
[0096] In addition, the modified liquid is mixed with the composite material and distilled water in a mass ratio of 0.22:1.
[0097] The composite material is a mixture of aluminum phosphate and sodium phosphate in a mass ratio of 1:0.4.
[0098] The preparation process of functional additives is as follows:
[0099] Aluminum nitride, oxalic acid and nickel acetate tetrahydrate were placed in a stirring device and mixed thoroughly in a mass ratio of 1:0.36:0.24, and then placed in a grinding device and ground for 30 minutes to obtain a grinding product;
[0100] The obtained ground product is placed in a nitrogen atmosphere and subjected to a two-stage high temperature treatment to obtain a functional additive;
[0101] Among them, the two-stage high temperature process is as follows:
[0102] The first stage: heating to 420℃ at a heating rate of 5℃ / min and keeping the temperature for 30min;
[0103] The second stage: heating to 500°C at a heating rate of 8°C / min and keeping the temperature for 50 minutes.
[0104] Furthermore, the sintering aid is a mixture of nano magnesium oxide and nano zirconium dioxide in a mass ratio of 1:0.12.
[0105] In addition, this embodiment also provides a method for preparing the above-mentioned graphite boat saturated film layer structure, which is characterized by comprising the following steps:
[0106] Step 1: accurately weigh the adhesive, compound nano powder, functional filler, functional additive and sintering agent, and put the adhesive, compound nano powder, functional filler, functional additive and sintering agent into a mixing device for mixing and stirring to obtain a film material;
[0107] Step 2: coating the obtained film material on the surface of the cleaned graphite boat body, then heating to 120° C. and keeping the temperature for 8 minutes;
[0108] The coating thickness is 0.8 mm.
[0109] Step 3: In a vacuum environment of 12 Pa, the temperature is increased to 740°C at a heating rate of 140°C / min, and the temperature is kept for 10 minutes;
[0110] Step 4: Heat the temperature to 1740°C at a heating rate of 100°C / min using nitrogen, and keep the temperature and pressure for 140 minutes under a hot pressing pressure of 30 MPa. After cooling, the test process is completed.
[0111] Comparative Example 1: The difference from Example 1 is that in this example, an equal amount of silicon is used to replace the compound nanopowder.
[0112] Comparative Example 2: The difference from Example 1 is that in this example, an equal amount of aluminum oxide is used to replace the functional filler.
[0113] Comparative Example 3: The difference from Example 1 is that in this example, an equal amount of aluminum nitride is used to replace the functional additive.
[0114] Comparative Example 4: The difference from Example 1 is that this example does not contain a sintering aid.
[0115] Performance test: The graphite boat saturated film layer samples provided in Examples 1 to 3 and Comparative Examples 1 to 4 are marked as Examples 1 to 3 and Comparative Examples 1 to 4, respectively; and the relevant properties of the graphite boat saturated film layers provided in Examples 1 to 3 and Comparative Examples 1 to 4 are tested as follows:
[0116] 1. Color defect rate test: The test method is to use the graphite boats obtained from each group to produce PERC solar cells in the same furnace tube, and count the number and total number of color defects in each graphite boat. Color defect rate = number / total number × 100%.
[0117] 2. Anti-destruction test: The test method is to process the graphite boat according to the size of 130*35*10, clamp the boat to be tested at different electrode positions of the same evaporation equipment, and control the same evaporation conditions, that is, control the voltage and wire feeding speed to be the same, and gradually increase the voltage in advance according to the gradient boosting method. When the evaporation is stable, the power is controlled at about 3KW, the vacuum degree is controlled at more than 10-2mba, and the wire feeding speed is controlled at 400mm / min for continuous evaporation. The diameter of the aluminum wire is 1.8mm, and the failure time is recorded. The failure of the evaporation boat is judged as follows: after increasing the evaporation power, the boat cannot be lit, the aluminum wire cannot melt or evaporate, resulting in aluminum accumulation, or a more serious boiling occurs on the boat surface, the wire feeding is stopped, and the failure time is recorded.
[0118] The obtained test data are recorded in Table 1 and Table 2 below:
[0119] Table 1 Test results of color defect rate of each group
[0120] Group EI dark film defect rate (%) Example 1 Group 0.02 Example 2 Group 0.03 Example 3 Group 0.05 Comparison group 1 13.82 Comparison of 2 groups 14.55 Comparison of 3 groups 15.18 Comparison of 4 groups 13.78
[0121] Table 2 Anti-destruction test results of each group
[0122] Group Failure time (h) Example 1 Group 9.2 Example 2 Group 9.0 Example 3 Group 9.2 Comparison group 1 5.2 Comparison of 2 groups 5.8 Comparison of 3 groups 6.1 Comparison of 4 groups 5.0
[0123] By comparing and analyzing the relevant data in Table 1 and Table 2, it can be seen that the graphite boat saturated film layer structure prepared by the present invention not only has excellent corrosion resistance, but also has the effect of reducing the product defect rate when used, effectively ensuring its quality. This shows that the graphite boat saturated film layer structure and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion.
[0124] The saturated film layer structure of a graphite boat provided by the present invention comprises a graphite boat body and a saturated film layer arranged on the surface of the graphite boat body, wherein the saturated film layer uses adhesive, compounded nano powder, functional filler, functional auxiliary agent and sintering aid as raw materials, wherein the compounded nano powder is compounded by mixing silicon, molybdenum and chromium, the functional filler is compounded by mixing modified filler and alumina, the functional auxiliary agent is obtained by mixing and grinding aluminum nitride, oxalic acid and nickel acetate tetrahydrate, and then subjecting them to high temperature treatment in a nitrogen atmosphere using a two-stage high temperature method, and the sintering aid is obtained by mixing nano magnesium oxide and nano zirconium dioxide; the saturated film layer structure of a graphite boat provided by the present invention is obtained by putting adhesive, compounded nano powder, functional filler, functional auxiliary agent and sintering aid into a mixing device for mixing and stirring to obtain a film material, and then coating the obtained film material on the surface of the cleaned graphite boat body, and then sintering, cooling, and then undergoing an inspection process. The graphite boat saturated film layer structure prepared by the present invention not only has excellent corrosion resistance, but also has the effect of reducing product defect rate when used, thereby effectively ensuring its quality.
[0125] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0126] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A graphite boat saturated film structure, characterized in that: It comprises a graphite boat body and a saturated film layer arranged on the surface of the graphite boat body; The saturated film layer is composed of the following raw materials in parts by weight: 20 to 30 parts of adhesive, 3 to 6 parts of compound nano powder, 3 to 5 parts of functional filler, 2 to 4 parts of functional additive and 4 to 7 parts of sintering aid.
2. The graphite boat saturated film structure according to claim 1, characterized in that: The adhesive is selected from any one of epoxy resin adhesive and acrylic adhesive.
3. The graphite boat saturated film structure according to claim 1, characterized in that: The compound nano powder is prepared by mixing silicon, molybdenum and chromium in a mass ratio of 1:0.12-0.22:0.08-0.
13.
4. The graphite boat saturated film structure according to claim 1, characterized in that: The functional filler is prepared by mixing and compounding the modified filler and alumina in a mass ratio of 1:0.08-0.
28.
5. The graphite boat saturated film structure according to claim 4, characterized in that: The preparation process of the modified filler is as follows: Place an appropriate amount of carbon nitride powder in an appropriate amount of modified liquid at a solid-liquid ratio of 0.01-0.12 g / mL, stir at 30-50 r / min for 10-14 min, then ultrasonically treat for 20-30 min, then treat at a water bath temperature of 25-30 min and 120-140 r / min for 100-120 min, and after suction filtration, wash the filter cake with anhydrous ethanol and deionized water for 2-4 times respectively; After washing, the filler is placed in a vacuum drying device at 60-70°C and dried for 12-14 hours to obtain a modified filler.
6. The graphite boat saturated film structure according to claim 5, characterized in that: The modified liquid is prepared by mixing the composite material and distilled water in a mass ratio of 0.12 to 0.22:
1.
7. The graphite boat saturated film structure according to claim 6, characterized in that: The composite material is prepared by mixing aluminum phosphate and sodium phosphate in a mass ratio of 1:0.2-0.
4.
8. The graphite boat saturated film structure according to claim 1, characterized in that: The preparation process of the functional additive is as follows: Aluminum nitride, oxalic acid and nickel acetate tetrahydrate are placed in a stirring device and mixed thoroughly in a mass ratio of 1:0.26-0.36:0.12-0.24, and then placed in a grinding device and ground for 20-30 minutes to obtain a grinding product; The obtained ground product is placed in a nitrogen atmosphere and subjected to a two-stage high temperature treatment to obtain a functional additive; Among them, the two-stage high temperature process is as follows: The first stage: heating to 420℃ at a heating rate of 4-5℃ / min, and heat preservation for 20-30min; The second stage: heating to 500°C at a heating rate of 8°C / min and keeping warm for 40 to 50 minutes.
9. The graphite boat saturated film structure according to claim 1, characterized in that: The sintering aid is prepared by mixing nano magnesium oxide and nano zirconium dioxide in a mass ratio of 1:0.06-0.
12.
10. The method for preparing a graphite boat saturated film structure according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: accurately weigh the adhesive, compound nano powder, functional filler, functional additive and sintering agent, and put the adhesive, compound nano powder, functional filler, functional additive and sintering agent into a mixing device for mixing and stirring to obtain a film material; Step 2: coating the obtained film material on the surface of the cleaned graphite boat body, then heating to 105-120° C. and keeping the temperature for 5-8 minutes; Step 3: In a vacuum environment of 6-12 Pa, the temperature is raised to 720-740° C. at a heating rate of 120-140° C. / min, and the temperature is kept for 6-10 minutes; Step 4: Heat the temperature to 1720-1740°C at a heating rate of 80-100°C / min using nitrogen, and keep the temperature and pressure for 120-140 minutes under a hot pressing pressure of 28-30 MPa. After cooling, the product can be inspected.
Citation Information
Patent Citations
Graphite boat saturated film structure and preparation method thereof
CN117702089A
Graphite evaporation boat and preparation method thereof
CN117800766A
Graphite boat saturated film layer structure and graphite boat for PERC solar cell
CN215163120U
BN-coated graphite material
JP1988035479A
Ceramics coating graphite and manufacturing method
JP2009227491A