Aluminum-coated aluminum-lithium alloy, vapor deposition method thereof and solid propellant containing aluminum-coated aluminum-lithium alloy

By forming a dense aluminum coating film and alumina coating film on the surface of aluminum-lithium alloy, the problems of difficulty in ignition and poor stability of aluminum powder propellant are solved, the specific impulse and stability of rocket propellant are improved, and the combustion performance is ensured. and compatibility.

CN118908791APending Publication Date: 2024-11-08XIANGTAN UNIV

Patent Information

Application Number
CN202410984493.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

As a rocket propellant, aluminum powder has problems such as ignition difficulties, incomplete combustion and specific impulse loss, and aluminum-lithium alloys are prone to aging in humid environments and have poor stability.

Method used

By forming a dense aluminum coating film and an alumina coating film on the surface of the aluminum-lithium alloy, an aluminum-clad aluminum-lithium alloy is prepared by vapor deposition method to control the thickness and mass of the coating film, prevent water vapor erosion and maintain combustion performance.

Benefits of technology

The stability and combustion performance of aluminum-lithium alloys are improved, the problem of coating thickness affecting combustion is avoided, compatibility with propellant is ensured, and suitable for high lithium content alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908791A_ABST
    Figure CN118908791A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum-coated aluminum-lithium alloy, a vapor deposition method thereof and a solid propellant containing the aluminum-coated aluminum-lithium alloy, and the aluminum-coated aluminum-lithium alloy sequentially comprises an aluminum-lithium alloy core, an aluminum coating film and an aluminum oxide coating film from inside to outside; the total thickness of the aluminum coating film and the aluminum oxide coating film is 0.5-1 [mu] m; specifically, trimethylaluminum is used, and an organic metal chemical vapor deposition method is adopted, so that the coating film is formed on the surface of the aluminum-lithium alloy; the aluminum-coated aluminum lithium alloy disclosed by the invention can be added into a solid propellant. The surface of the aluminum-lithium alloy is coated with aluminum to form a compact coating film, so that the influence of external water vapor on the aluminum-lithium alloy is effectively prevented and isolated, and the stability of the aluminum-lithium alloy in the storage process is maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal powder material preparation, and in particular to an aluminum-coated aluminum-lithium alloy, a vapor deposition method thereof, and a solid propellant containing the same. Background Art

[0002] Rocket propellants are substances that are ejected from rocket engines in large quantities in the form of fluid jets to generate thrust for propulsion. They are divided into liquid propellants and fixed propellants. Aluminum powder is usually used in solid propellants to provide combustion heat, thereby increasing the thrust of the rocket. However, the presence of an oxide film on the surface of aluminum powder makes it difficult to ignite, and when the propellant containing aluminum powder burns, the actual specific impulse of the aluminum powder will be lost to a certain extent due to the melting and agglomeration of aluminum powder particles on the combustion end surface and incomplete combustion. Summary of the invention

[0003] The present application provides an aluminum-coated aluminum-lithium alloy, a vapor deposition method thereof, and a solid propellant containing the same, to solve the related defect problems existing when aluminum powder is used as a propellant.

[0004] In order to solve the problems existing when using aluminum powder, the inventors of this application have found through research that aluminum-lithium alloy can reduce the ignition temperature of the propellant, and the presence of lithium can also change the structure of the dense oxide film on the aluminum surface, so that the contact performance with the oxidant in the propellant is improved, thereby making the powder burn more fully and improving the specific impulse of the propellant. However, aluminum-lithium alloy is greatly affected by environmental factors during storage, especially in a humid environment, and is easy to react with water in the air, which accelerates its aging and has poor stability. Therefore, how to improve the stability of aluminum-lithium alloy is very important.

[0005] The inventors of this application have tried to improve the stability of aluminum-lithium alloys, such as: 1. Sol method, using organic matter to form a coating film on the surface of alloy powder for protection, but the film formed by the sol method is not strong and easy to fall off, and the organic matter used is easy to affect the compatibility with the propellant, and it is difficult to use this method to achieve coating of aluminum-lithium alloys with high lithium content. 2. Using the vapor deposition method, the technical inspiration given by the relevant technology is to use carbonyl nickel to vapor deposit metal powder, but carbonyl nickel is highly toxic, and the calorific value of the formed metal nickel protective layer is low, which will also affect the combustion performance and has defects.

[0006] Through the continuous creative work of the inventors of this application:

[0007] In a first aspect, the present application provides an aluminum-coated aluminum-lithium alloy, which comprises, from the inside to the outside, an aluminum-lithium alloy core, an aluminum coating film, and an aluminum oxide coating film; the total thickness of the aluminum coating film and the aluminum oxide coating film is 0.5 to 1 μm.

[0008] The present application forms a relatively dense coating film by coating aluminum on the surface of the aluminum-lithium alloy, thereby effectively preventing and isolating the influence of external water vapor on the aluminum-lithium alloy and maintaining the stability of the aluminum-lithium alloy during storage. The present application controls the thickness of the coating film to be 0.5 to 1 μm. The controlled thickness meets the isolation requirements while not generating an excessively thick coating film that would cause subsequent ignition difficulties and affect combustion performance.

[0009] In a possible implementation of the present application, the total mass of the aluminum coating film and the aluminum oxide coating film is 3-15% of the mass of the aluminum-lithium alloy.

[0010] The present application controls the total mass of the coating to be 3-15% of the mass of the aluminum-lithium alloy, which not only meets the insulation requirements but also avoids the generation of an overly thick and heavy coating film that would cause difficulty in subsequent ignition and affect combustion performance, and controls costs to a certain extent.

[0011] In a possible implementation of the present application, the aluminum content in the aluminum-lithium alloy is 90-95 wt.%, and the lithium content is 5-10 wt.%. The aluminum-lithium alloy with such content has good combustion performance and relatively high stability.

[0012] In a second aspect, the present application provides a vapor deposition method for the above-mentioned aluminum-coated aluminum-lithium alloy, using trimethylaluminum and an organic metal chemical vapor deposition method to form an aluminum coating film on the surface of the aluminum-lithium alloy.

[0013] In a possible implementation of the present application, the vapor deposition method includes the following steps:

[0014] S1, placing the aluminum-lithium alloy into a reactor, filling the reactor with an inert gas to exhaust air, and forming a positive pressure environment in the reactor;

[0015] S2, heating the reactor to 150-200° C., and continuously introducing an inert gas during the heating process;

[0016] S3, ensuring an inert gas environment, and introducing trimethylaluminum vapor into the reactor, and heat-retaining the reaction at 200-250° C.;

[0017] S4. Ensure an inert gas environment, raise the temperature of the reactor to 350-500°C at a uniform rate, and continue to maintain the temperature for 1-1.5 hours after heating.

[0018] In a possible implementation of the present application, in S2, the reactor is heated to 150-200° C. at a rate of 5-10° C. / min, and the inert gas is introduced at a flow rate of 1-2 L / min.

[0019] In a possible implementation of the present application, in S3, trimethylaluminum vapor is loaded with an inert gas, and the reaction is kept at 200-250° C. for 30-60 min, and the loading flow rate of the inert gas is 1-2 L / min.

[0020] Through multiple creative experiments and taking into account the deposition rate, the present applicant has found that under the experimental conditions of the above parameters, the generated coating layer is uniform and dense, and can achieve an excellent coating protection effect.

[0021] In a possible implementation of the present application, the temperature in S4 is raised to 350-500° C. at a rate of 5-10° C. / min, and the flow rate of the inert gas loaded into trimethylaluminum is 1.5-2 L / min.

[0022] In a third aspect, the present application provides a solid propellant, the components of which include the aluminum-coated aluminum-lithium alloy of the first aspect or the aluminum-coated aluminum-lithium alloy produced by the method of the second aspect.

[0023] This application has the following beneficial effects:

[0024] 1. Aluminum coating is used to coat the original components of the aluminum-lithium alloy, which will not reduce the combustion performance of the aluminum-lithium alloy after coating.

[0025] 2. By forming a dense alumina coating on the surface of the aluminum-lithium alloy, the aluminum-lithium alloy is coated and stabilized, effectively preventing and isolating the influence of external environmental water vapor on the aluminum-lithium alloy, improving the antioxidant performance, ensuring that the aluminum-lithium alloy is not corroded during storage, and having good compatibility with other components of the propellant.

[0026] 3. The coating layer prepared by the vapor deposition method of the present application has an appropriate thickness and quality, which not only ensures the insulation performance, but also avoids the problem of overall combustion performance being affected by factors such as the thickness of the coating film. The calorific value and combustion performance of the aluminum-lithium alloy after coating are not affected.

[0027] 4. Compared with the sol method, the vapor deposition method of the present application can not only form a continuous, firm and dense coating film, but also can coat alloys with high lithium content because it does not need to be carried out in a solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the structure of aluminum-coated aluminum-lithium alloy;

[0029] Figure 2 This is a scanning electron microscope image of aluminum-lithium alloy;

[0030] Figure 3 This is a scanning electron microscope image of aluminum-coated aluminum-lithium alloy. DETAILED DESCRIPTION

[0031] In order to enable a more detailed understanding of the features and technical contents of the embodiments of the present application, the following is a detailed explanation in conjunction with the implementation of the embodiments of the present application.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.

[0033] In the following description, reference is made to “some embodiments”, which describe a subset of all possible embodiments, but it will be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.

[0034] It should also be pointed out that the terms "first\second\third" involved in the embodiments of the present application are only used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged in a specific order or sequence where permitted, so that the embodiments of the present application described here can be implemented in an order other than that illustrated or described here.

[0035] It should be understood that the "embodiments of the present application" or "the aforementioned embodiments" mentioned throughout the specification mean that specific features, structures or characteristics related to the embodiments are included in at least one embodiment of the present application. Therefore, "in the embodiments of the present application" or "in the aforementioned embodiments" appearing throughout the specification may not necessarily refer to the same embodiment. In addition, these specific features, structures or characteristics can be combined in one or more embodiments in any suitable manner. In the various embodiments of the present application, the size of the sequence number of the above-mentioned processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application. The above-mentioned sequence numbers of the embodiments of the present application are for description only and do not represent the advantages and disadvantages of the embodiments.

[0036] It should be noted that, for the description of the same steps and the same contents in this embodiment as those in other embodiments, reference can be made to the description in other embodiments and will not be repeated here.

[0037] The methods disclosed in several method embodiments provided in this application can be arbitrarily combined without conflict to obtain new method embodiments.

[0038] The features disclosed in several product embodiments provided in this application can be arbitrarily combined without conflict to obtain new product embodiments.

[0039] The features disclosed in several method or device embodiments provided in this application can be arbitrarily combined without conflict to obtain new method embodiments or device embodiments.

[0040] Example 1

[0041] An aluminum-coated aluminum-lithium alloy uses trimethylaluminum and adopts an organic metal chemical vapor deposition method to form an aluminum coating layer on the surface of the aluminum-lithium alloy.

[0042] C3H9Al (l) →C3H9Al (g) +Al-Li alloy powder →Al-coated Al-Li alloy powder + CH3↑

[0043] Prepared by the following method:

[0044] S1. 100 g of an aluminum-lithium alloy Al-10Li having an aluminum content of 90 wt.% and a lithium content of 10 wt.% is placed in a reactor, and inert argon gas is filled into the reactor to exhaust air, so that the reactor forms a positive pressure environment;

[0045] S2, heating the reactor to 200°C at a rate of 5°C / min, and introducing an inert gas at a flow rate of 1 L / min;

[0046] S3, using inert gas argon to load trimethylaluminum vapor, and keeping the temperature at 200° C. for 30 min, the loading flow rate of the inert gas argon is 1 L / min;

[0047] S4, the flow rate of the inert gas argon loaded with trimethylaluminum was adjusted to 1.5 L / min, the reactor was heated to 400°C at a rate of 5°C / min, and the temperature was maintained at 400°C for 1 hour after the temperature was raised;

[0048] S5. Continue to introduce inert gas argon for temperature reduction protection, and adjust the flow rate of inert gas argon to 1L / min;

[0049] S6. Performing a passivation treatment on the product to form a passivation film on the surface.

[0050] The aluminum-coated aluminum-lithium alloy obtained by the above method has a structural schematic diagram as shown in Figure 1 As shown, from the inside to the outside, it includes an aluminum-lithium alloy core, an aluminum coating film, and an aluminum oxide coating film; the total thickness of the aluminum coating film and the aluminum oxide coating film is 0.5 μm, and the total mass of the aluminum coating film and the aluminum oxide coating film is 3% of the mass of the aluminum-lithium alloy.

[0051] Figure 2 This is a scanning electron microscope image of a pure aluminum-lithium alloy, showing the metallographic structures such as "grooves" and "channels" on its surface. Figure 3This is a scanning electron microscope image of the aluminum-lithium alloy after aluminum coating. It can be seen that the grooves on the surface of the aluminum-lithium alloy are completely coated, and the metallographic structure of the original aluminum-lithium alloy powder does not exist. Therefore, it is explained that the coating layer formed by the coating method of the present application is dense, which can improve the stability while ensuring that the direct viscosity of the powder is small, and will not cause the problem of agglomeration between powders affecting the subsequent use effect in solid propellants.

[0052] Example 2

[0053] An aluminum-coated aluminum-lithium alloy uses trimethylaluminum and adopts an organic metal chemical vapor deposition method to form an aluminum coating layer on the surface of the aluminum-lithium alloy.

[0054] Prepared by the following method:

[0055] S1. Take 150g of Al-10Li aluminum-lithium alloy and put it into a reactor. Fill the reactor with inert gas argon to expel air and form a positive pressure environment in the reactor.

[0056] S2, heating the reactor to 150°C at a rate of 5°C / min, continuously introducing inert gas argon during the heating process, and the inert gas argon introduction rate is 1 L / min;

[0057] S3, using inert gas argon to load trimethylaluminum vapor, and keeping the temperature at 200° C. for 30 min, the loading flow rate of the inert gas argon is 1 L / min;

[0058] S4, the flow rate of the inert gas argon loaded with trimethylaluminum was adjusted to 0.5 L / min, the reactor was heated to 500° C. at a rate of 5° C. / min, and the temperature was maintained at 500° C. for 0.5 h after the temperature was raised;

[0059] S5. Continue to introduce inert gas argon for temperature reduction protection, and adjust the flow rate of inert gas argon to 1L / min;

[0060] S6. Performing a passivation treatment on the product to form a passivation film on the surface.

[0061] The aluminum-coated aluminum-lithium alloy obtained by the above method includes, from the inside to the outside, an aluminum-lithium alloy core, an aluminum coating film, and an aluminum oxide coating film; the total thickness of the aluminum coating film and the aluminum oxide coating film is 0.2um, and the total mass of the aluminum coating film and the aluminum oxide coating film is 1% of the mass of the aluminum-lithium alloy.

[0062] Example 3

[0063] An aluminum-coated aluminum-lithium alloy uses trimethylaluminum and adopts an organic metal chemical vapor deposition method to form an aluminum coating layer on the surface of the aluminum-lithium alloy.

[0064] Prepared by the following method:

[0065] S1. Take 100g of Al-10Li aluminum-lithium alloy and put it into a reactor. Fill the reactor with inert gas argon to expel air and form a positive pressure environment in the reactor.

[0066] S2, heating the reactor to 200°C at a rate of 10°C / min, continuously introducing inert gas argon during the heating process, and the introduction rate of inert gas argon is 1 L / min;

[0067] S3, using inert gas argon to load trimethylaluminum vapor, and keeping the temperature at 200° C. for 30 min, the loading flow rate of the inert gas argon is 1 L / min;

[0068] S4, the flow rate of the inert gas argon loaded with trimethylaluminum is adjusted to 1 L / min, the reactor is heated to 450°C at a rate of 10°C / min, and the temperature is maintained at 450°C for 1.5 hours after the temperature is raised;

[0069] S5. Continue to introduce inert gas argon for temperature reduction protection, and adjust the flow rate of inert gas argon to 1L / min;

[0070] S6. Performing a passivation treatment on the product to form a passivation film on the surface.

[0071] The aluminum-coated aluminum-lithium alloy obtained by the above method includes, from the inside to the outside, an aluminum-lithium alloy core, an aluminum coating film, and an aluminum oxide coating film; the total thickness of the aluminum coating film and the aluminum oxide coating film is 1.0um, and the total mass of the aluminum coating film and the aluminum oxide coating film is 12% of the mass of the aluminum-lithium alloy.

[0072] The aluminum-coated aluminum-lithium alloy prepared by the method of the above embodiment can be added to the solid propellant. The amount of the aluminum-coated aluminum-lithium alloy added to the solid propellant is 10-20wt.%. The solid propellant can adopt the components with mass contents shown in the following table:

[0073] HTPB hydroxyl-terminated polybutadiene AP Ammonium Perchlorate RDX Cyclotrimethylene trinitramine Aluminum-clad aluminum-lithium alloy 10-12 60-70 0-10 10-20

[0074] For example, the solid additive may be composed of the following ingredients: 19 wt. % of aluminum-coated aluminum-lithium alloy prepared by the above method, 12 wt. % of HTPB terminal hydroxyl polybutadiene, 61 wt. % of AP ammonium perchlorate, and 8 wt. % of RDX cyclotrimethylene trinitramine.

[0075] In order to compare and verify the effects of the embodiments of the present application, other raw materials are used to obtain the coating film.

[0076] Comparative Example 1

[0077] An iron coating is formed on the surface of the same aluminum-lithium alloy by using an iron target as a raw material and a magnetron sputtering method.

[0078] Comparative Example 2

[0079] A silane coupling agent is used as a raw material and a sol coating method is adopted to form an iron coating film on the surface of the same aluminum-lithium alloy.

[0080] Comparative Example 3

[0081] Carbonyl nickel was used as a raw material, and a nickel coating was formed on the surface of the same aluminum-lithium alloy using the same method as in Example 1.

[0082] Comparative Example 4

[0083] Only aluminum-lithium alloy is used without any coating on its surface.

[0084] The performance of the aluminum-coated aluminum-lithium alloys of Examples 1-3, the aluminum-lithium alloys coated with other raw materials of Comparative Examples 1-3, and the pure aluminum-lithium alloy of Comparative Example 4 were tested by oxygen bomb tests. The results showed that:

[0085]

[0086] From the above experimental results, it can be seen that the iron coating and nickel coating reduce the calorific value and affect the combustion performance, and the silicon coating directly inhibits the combustion. However, after the aluminum-lithium alloy is coated with Al, its calorific value is not affected and is equivalent to the calorific value of the uncoated pure aluminum-lithium alloy, which ensures the stability of the aluminum-lithium alloy and the combustion performance.

[0087] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. An aluminum-coated aluminum-lithium alloy, characterized in that: From the inside to the outside, it includes an aluminum-lithium alloy core, an aluminum coating film, and an aluminum oxide coating film; The total thickness of the aluminum coating film and the aluminum oxide coating film is 0.5 to 1 μm.

2. The aluminum-clad aluminum-lithium alloy according to claim 1, characterized in that The total mass of the aluminum coating film and the aluminum oxide coating film is 3-15% of the mass of the aluminum-lithium alloy.

3. The aluminum-clad aluminum-lithium alloy according to claim 1, characterized in that The aluminum content in the aluminum-lithium alloy is 90-95 wt.% 、 The content of lithium is 5 to 10 wt.%.

4. A vapor deposition method for aluminum-coated aluminum-lithium alloy as claimed in any one of claims 1 to 3, characterized in that: An aluminum coating is formed on the surface of an aluminum-lithium alloy by using trimethylaluminum and an organic metal chemical vapor deposition method.

5. The vapor deposition method according to claim 4, characterized in that The vapor deposition method comprises the following steps: S1, placing the aluminum-lithium alloy into a reactor, filling the reactor with an inert gas to exhaust air, and forming a positive pressure environment in the reactor; S2, heating the reactor to 150-200° C., and continuously introducing an inert gas during the heating process; S3, ensuring an inert gas environment, and introducing trimethylaluminum vapor into the reactor, and heat-retaining the reaction at 200-250° C.; S4. Ensure an inert gas environment, raise the temperature of the reactor to 350-500°C at a uniform rate, and continue to maintain the temperature for 1-1.5 hours after heating.

6. The vapor deposition method according to claim 5, characterized in that In step S2, the reactor is heated to 150-200° C. at a rate of 5-10° C. / min, and the inert gas is introduced at a flow rate of 1-2 L / min.

7. The method according to claim 5, characterized in that In step S3, inert gas is used to load trimethylaluminum vapor, and the reaction is kept at 200-250° C. for 30-60 minutes. The loading flow rate of the inert gas is 1-2 L / min.

8. The vapor deposition method according to claim 5, characterized in that In step S4, the temperature is raised to 350-500° C. at a rate of 5-10° C. / min, and the flow rate of the inert gas loaded into trimethylaluminum is 1.5-2 L / min.

9. A solid propellant, characterized in that: Its components include the aluminum-clad aluminum-lithium alloy as described in any one of claims 1 to 3 or the aluminum-clad aluminum-lithium alloy prepared by the vapor deposition method as described in any one of claims 4 to 8.

Citation Information

Patent Citations

  • Method for preparing Al-Li master alloy through electrodeposition with lithium oxide serving as raw material at near room temperature

    CN106967998A

  • Preparation method of light high-strength powder metallurgy aluminum-lithium alloy

    CN112626365A

  • Method for stabilizing aluminum-lithium alloy powder through organic matter coating

    CN116422878A

  • Method for realizing aluminum alloy reaction diffusion bonding by depositing copper nano layer on interface

    CN118081054A

  • Metal deposition

    GB1594399A

Cited By

  • Aluminum-lithium alloy efficient passivation process and obtained high-stability powder

    CN119794338A

  • An efficient passivation process for aluminum-lithium alloys and the resulting high-stability powder