Polymer, preparation method thereof and application of polymer as anion exchange membrane

By using polymers with nitrogen heterocyclic structure in anion exchange membrane and combining with specific synthesis methods, the existing membrane's performance problems in long-term reactions in high temperatures are solved, and high conductivity, current density and mechanical stability are achieved. Improved, suitable for electrolyzing water to produce hydrogen and CO2 conversion.

CN118909214APending Publication Date: 2024-11-08CHINA CHEM TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410979432.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing anion exchange membrane has problems such as low conductivity, poor mechanical strength, short cycle life and small current density during long-term reactions at high temperatures, which limits its widespread use in industrial applications.

Method used

Using a novel polymer whose structure contains saturated or unsaturated alumina heterocycles as the main chain, high conductivity and Anion exchange membrane with high current density.

Benefits of technology

The conductivity and current density of the anion exchange membrane are improved, its mechanical stability is enhanced, cycle life is extended, and performance in electrolyzed water hydrogen production and CO2 conversion is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909214A_ABST
    Figure CN118909214A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer, a preparation method thereof and application of the polymer as an anion exchange membrane. The polymer has a structure as shown in a formula I: # imgabs0 #, the polymer at least has high conductivity when being used as an anion exchange membrane, and the current density of an electrolytic tank is higher under the same voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymers, and in particular relates to a polymer and a preparation method thereof and application thereof as an anion exchange membrane (AEM). Background Art

[0002] Anion exchange membrane water electrolysis is a new green hydrogen production technology that has emerged in recent years. Many research institutions are actively developing it. The main reason is the attention from all walks of life to downstream hydrogen fuel cells. Compared with other traditional electrolysis technologies, this technology has low cost and good performance. Anion exchange membrane (AEM) is a polymer electrolyte membrane used in various applications involving the transport of anions (negatively charged ions). AEM can selectively conduct anions while blocking the passage of cations (positively charged ions).

[0003] Alkaline electrolyzed water occupies a dominant position in the current industrial market due to its low cost and highest technological maturity, but its energy efficiency is relatively low; proton exchange membrane electrolyzed water mostly uses highly active precious metals as catalysts and needs to maintain its excellent performance under highly corrosive conditions, and the overall cost is relatively high.

[0004] The main difference between alkaline water electrolysis and AEM water electrolysis is that anion exchange membrane (quaternary ammonium ion exchange membrane) is used to replace the traditional diaphragm (asbestos, PPS, etc.) in alkaline electrolysis. In contrast, anion exchange membrane water electrolysis can use dilute alkaline solution or pure water as the electrolyte, use relatively cheap anion exchange membrane and highly active non-precious metal catalyst, effectively reduce the energy consumption of water electrolysis, and greatly reduce the input cost, which has great market competitiveness; but because the thermal stability and chemical stability of the anion exchange membrane have not yet reached the commercial level, and during the high temperature and long-term reaction process, the catalyst in the membrane electrode assembly may dissolve and fall off or the membrane may degrade, and the ion transmission capacity may be weakened. At present, most AEM membranes have low conductivity (<100mS / cm@60℃), poor mechanical strength (<30Mpa), poor cycle life (cycle 8000 hours, IEC decay greater than 5%) and / or low current density. How to prepare an anion exchange membrane with high conductivity, high current density and / or high mechanical stability has become a top priority for the development of the industry. Summary of the invention

[0005] In order to improve the above technical problems, the present invention provides a polymer having a structure as shown in Formula I:

[0006]

[0007] Wherein, A represents a saturated or unsaturated nitrogen heterocycle, such as a saturated or unsaturated nitrogen five-membered ring or nitrogen six-membered ring; further, the nitrogen atom on A may be substituted, such as by at least one C1-8 Alkyl or C 1-8 Alkoxy substituted, preferably with one or two C 1-4 Alkyl, C 1-4 Alkoxy substitution;

[0008] R 1 , R 2 and R 3 The same or different, independently selected from H, C 1-8 Alkyl, C 1-8 Alkoxy;

[0009] R 1 Attached to a carbon atom on ring A;

[0010] B - represents an anion, such as OH - .

[0011] According to an embodiment of the present invention, R 1 , R 2 and R 3 The same or different, independently selected from H, C 1-4 Alkyl, C 1-4 Alkoxy; in one embodiment, R 1 , R 2 and R 3 The same is selected from H, methyl, ethyl, propyl, butyl, methoxy or ethoxy.

[0012] According to an embodiment of the present invention, the nitrogen atom on A is substituted by two groups, for example, any two groups selected from methyl, ethyl, propyl, butyl, methoxy or ethoxy.

[0013] According to an embodiment of the present invention, A represents a saturated or unsaturated five-membered ring containing one nitrogen atom, a five-membered ring containing two nitrogen atoms, or a six-membered ring containing one nitrogen atom.

[0014] Illustratively, the A is provided by a compound of formula A below.

[0015] According to an embodiment of the present invention, the molecular weight of the polymer is 20,000 to 100,000 g / mol, such as 30,000 to 90,000 g / mol, 40,000 to 80,000 g / mol or 50,000 to 70,000 g / mol.

[0016] According to one embodiment of the present invention, the polymer has a structure as shown in Formula I-1:

[0017]

[0018] R 4 , R5 The same or different, independently selected from H, C 1-8 Alkyl, C 1-8 Alkoxy, preferably C 1-4 Alkyl, C 1-4 Alkoxy, exemplified by methyl, ethyl or propyl;

[0019] According to an exemplary embodiment of the present invention, the polymer has a structure as shown in Formula I-2:

[0020]

[0021] The present invention also provides a method for preparing the above polymer, comprising: soaking the polymer of formula D in an alkaline solution to obtain a polymer of formula I;

[0022]

[0023] wherein X represents a halogen, such as F, Cl, Br or I;

[0024] For example, the alkaline solution is a strong alkaline solution, such as a sodium hydroxide solution or a potassium hydroxide solution;

[0025] For example, the reaction soaking temperature is 40-60° C., and the time is not less than 10 hours.

[0026] According to an embodiment of the present invention, the preparation of the polymer of formula D comprises: reacting the polymer of formula C with a halogenated alkyl R 5 X is reacted in NMP, or in a system further adding DMSO, to obtain a polymer of formula D;

[0027]

[0028] According to an embodiment of the present invention, the alkyl halide R 5 X may be methyl iodide;

[0029] According to an embodiment of the present invention, the alkyl halide R 5 The molar ratio of X to the polymer structural unit of formula C is (2-5):1, for example 2:1, 3:1, 4:1 or 5:1;

[0030] According to an embodiment of the present invention, the reaction temperature is 60-80°C and the reaction time is 5-12 hours;

[0031] According to an embodiment of the present invention, the polymer of formula C may be first added to NMP until it can no longer be dissolved, and then DMSO may be added thereto.

[0032] According to an embodiment of the present invention, the preparation of the polymer of formula C comprises: reacting a compound of formula A and a compound of formula B in a system of trifluoroacetic acid, trifluoromethanesulfonic acid (TFSA) and dichloromethane to obtain a polymer of formula C;

[0033]

[0034] According to an embodiment of the present invention, the compound of formula A can be selected from

[0035] R 4 'With R 4 the same or different, with the definitions shown above;

[0036] Preferably, R 1 For H, R 4 is H or methyl. According to an embodiment of the present invention, the compound of formula A, the compound of formula B and dichloromethane are first mixed, trifluoroacetic acid is added dropwise thereto, and after the trifluoroacetic acid is added dropwise, trifluoromethanesulfonic acid is added dropwise thereto;

[0037] Preferably, the mixing and dropping are both performed under stirring conditions; preferably, the stirring speed is less than 100 rpm;

[0038] Preferably, the mixing and dropping are carried out at 0-4°C (e.g., ice bath);

[0039] According to an embodiment of the present invention, after the trifluoromethanesulfonic acid is added dropwise, the system is placed at room temperature to react for 2-4 hours;

[0040] According to an embodiment of the present invention, after the reaction is completed, the product is immersed in a potassium carbonate solution, washed with deionized water until the filtrate is neutral, and dried to obtain the polymer of formula C.

[0041] According to an exemplary embodiment of the present invention, when the polymer has a structural unit as shown in Formula I-2, the preparation method thereof includes:

[0042] (1) reacting the compound of formula A-1 and the compound of formula B-1 in a system of trifluoroacetic acid, trifluoromethanesulfonic acid (TFSA) and dichloromethane at room temperature to obtain a polymer of formula C-1;

[0043]

[0044] (2) reacting the polymer of formula C-1 with methyl iodide in NMP or in a system further containing DMSO to obtain a polymer of formula D-1;

[0045]

[0046] (3) The polymer of formula D is reacted and soaked in an alkaline solution to obtain a polymer of formula I-2;

[0047]

[0048] The present invention also provides application of the polymer as an anion exchange membrane.

[0049] The invention also provides an anion exchange membrane prepared from the above polymer.

[0050] For example, the polymer is dissolved in a mixed solvent of dimethyl sulfoxide and alcohol to obtain a membrane solution with a solid content of 18-30wt%, and the anion exchange membrane is obtained by casting. The alcohol is not limited to one or more of ethanol, n-butanol, isopropanol, methanol, butanediol and pentanediol.

[0051] According to an embodiment of the present invention, the thickness of the anion exchange membrane is 60 to 80 microns.

[0052] The present invention also provides the above polymer or anion exchange membrane in the electrolysis of water to produce hydrogen or CO 2 Application in conversion.

[0053] Beneficial Effects

[0054] The polymer of the present invention uses a polynitrogen heterocycle combined with a diphenyl sulfone structure as a main chain structure, and proposes a polymer with a completely new main chain structure. The polymer, as an anion exchange membrane, has at least high conductivity, and at the same voltage, the current density of the electrolytic cell is higher. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 The conductivity of the membrane product and the commercial product of Example 1 varies with temperature;

[0056] Figure 2 The current density of the membrane product and the commercial product of Example 1 varies with voltage;

[0057] Figure 3 The appearance of the polymer of formula C-1 in Example 1 (left) and the appearance of the film product (right). DETAILED DESCRIPTION

[0058] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0059] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0060] Example 1

[0061] Step 1: Synthetic resin

[0062] Select 50mL three-necked flask, weigh 8.95g p-diphenyl sulfone (0.041mol) and add it, place glass flask in ice bath, add 8.6mL dichloromethane, and 5.0mL N-methyl-4-piperidone (0.042mol). Adopt polytetrafluoroethylene two-leaf stirring rod and 150W mechanical stirrer to slowly stir the system, make reactant and solvent mix evenly. Then add trifluoroacetic acid 2.0mL with dropper in reaction system, and keep the system less than 100 rev / min stirring state. After trifluoroacetic acid adds, select 50mL constant pressure dropping funnel, slowly add 30mL trifluoromethanesulfonic acid in system, 5-10min adds, and keep the system less than 100 rev / min stirring state. Can observe the change of system color and solid state. Before system does not add trifluoromethanesulfonic acid, it is clear transparent solution, along with the adding of trifluoromethanesulfonic acid, system gradually becomes pink, and is accompanied by precipitation generation. With the further addition of trifluoromethanesulfonic acid, the system begins to change from pink to brown. After the addition of trifluoromethanesulfonic acid, remove the ice bath and slowly return to room temperature of 20-25°C. After reacting for 2-4 hours, the system turns brown, the viscosity increases significantly, and there is a climbing phenomenon, which indicates that the polymerization state is good. The polymerized product is clamped out with stainless steel tweezers and immersed in the prepared potassium carbonate solution. The product turns from brown to white. Ultrasonicate for 0.5 hours, break it with a juicer, soak it in potassium carbonate solution and stir it overnight, and wash it several times with deionized water the next day until the filtrate is neutral. Dry the product in an oven at 80°C for 24 hours to obtain yellow solid particles ( Figure 3 left figure), namely, the polymer of formula C-1.

[0063]

[0064] Step 2: Quaternization

[0065] Weigh 20g of the C-1 polymer raw material into a 500mL round-bottom flask, add 200mL NMP and heat to 70℃ to dissolve the polymer. If the potassium carbonate solution is thoroughly soaked during the synthesis of the C-1 polymer in the previous step, the tertiary amine on the piperidine is in a deprotonated state, that is, all the trifluoromethanesulfonic acid is reacted. At this time, the solubility of the polymer is not very good, and some of the polymer may not be dissolved in NMP, but this does not affect the subsequent quaternization reaction. When the polymer is dissolved in NMP to a certain extent and cannot be dissolved, add 100mL DMSO to it. The role of DMSO is not to promote the dissolution of the copolymer, but to improve the quaternization efficiency of iodomethane to piperidine. The higher the proportion of DMSO in the solvent, the higher the quaternization efficiency of iodomethane. After adding DMSO, wait until the temperature rises to 70℃, use a double-row pipe to drain the water in the system, half an hour, cool to room temperature, and add about twice the equivalent of the copolymer structural unit to the system. 6.0mL in total. This ratio is the amount of iodomethane used to ensure that the quaternization efficiency of the C-1 polymer can reach 85% or more, and can be adjusted accordingly according to actual conditions. If the C-1 polymer can be quickly and completely dissolved in NMP to obtain a completely clear and transparent solution, it means that a part of the piperidine is protonated by trifluoromethanesulfonic acid. At this time, more equivalents of iodomethane need to be added, such as 3-5 times, to ensure that the quaternization efficiency reaches 85% or more. After adding iodomethane, seal with a saline stopper, it can be observed that the undissolved C-1 polymer is rapidly dissolved, and the system gradually turns dark brown. This is because the quaternized C-1 polymer can be well dissolved in DMSO. The reaction temperature is raised to 70°C for 7 hours, and the reaction is completed to obtain a polymer of formula D-1.

[0066]

[0067] Step 3: Complete OH - Anion Exchange

[0068] The polymer of formula D-1 was placed in a 1M KOH solution at 50°C for OH - Anion exchange, reaction soaking for 24 hours. The obtained polymer is then dissolved in DMSO: ethanol (1:1, v / v) solvent, and the prepared membrane solution has a solid content in the range of 18-30%. On a casting machine, the film is cast to control the film thickness to 60-80 μm to obtain an anion exchange membrane (AEM) (see Figure 3 center right).

[0069]

[0070] Test Example 1

[0071] Conductivity is one of the electrochemical performance index parameters of the membrane, which directly determines the internal resistance and current density during the electrolysis process.

[0072] Using four-probe AC ​​impedance technology, -1 Hz-10 5 The impedance values ​​of the AEM in Example 1 and the AEM commercialized by Versogen in the United States were measured in the frequency range of Hz. The sample membranes were soaked in distilled water for 24 hours before testing and cut into uniform shapes (1 cm × 5 cm). The conductivity of the membrane (σ, mS / cm 2 ).

[0073]

[0074] The cross-sectional area of ​​the membrane is S (cm 2 ), the distance between the electrodes is L (cm), and the impedance of the membrane is recorded as R (Ω).

[0075] The conductivity at different temperatures is Figure 1 ( Figure 1 The implementation case is the AEM in Example 1, and the commercial sample is the AEM commercialized by Versogen Company of the United States. The specific values ​​are shown in Table 1.

[0076] Table 1

[0077] temperature <![CDATA[Conductivity of Example 1 AEM (mS / cm 2 )]]> <![CDATA[Conductivity of commercialized AEM (mS / cm 2 )]]> 40℃ 69 60 50℃ 98 93 60℃ 135 123 70℃ 142 135 80℃ 158 150

[0078] From the above, it can be seen that the conductivity of the AEM membrane of Example 1 is better than that of the commercial AEM at various temperatures.

[0079] Test Example 2

[0080] The test data of the single-chip electrolytic chamber is used to simulate the test data of the electrolytic cell to reflect the electrochemical performance of the membrane. The specific tests are as follows:

[0081] Electrolysis of water to produce hydrogen test fixture active area: 4cm 2 , film thickness 80 μm;

[0082] Test fixture temperature: 80℃;

[0083] Anode catalyst: NiFe (loading 6 mg / cm 2 );

[0084] Cathode catalyst: Pt / C (loading 1 mg / cm 2 );

[0085] Membrane samples: AEM of Example 1 and AEM commercialized by Versogen Corporation of the United States.

[0086] The current changes in the electrolysis chamber were observed by using an electrochemical workstation (CHI604) at voltages of (1.8 V, 2.0 V, 2.2 V). It can be seen that the current density of the AEM in Example 1 is (0.8 A / cm 2 , 3A / cm 2 , 4.5A / cm 2 ), which is better than the commercial AEM membrane (0.7A / cm 2 , 1.8A / cm 2 , 2.0 / cm 2 ), showing good electrochemical performance (see Figure 2 , Figure 2 The implementation case is the AEM in Example 1, and the commercial sample is the AEM commercialized by Versogen Company of the United States).

[0087] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polymer having a structure as shown in Formula I: in, A represents a saturated or unsaturated nitrogen heterocycle, such as a saturated or unsaturated nitrogen five-membered ring or nitrogen six-membered ring; further, the nitrogen atom on A may be substituted, such as by at least one C 1-8 Alkyl or C 1-8 Alkoxy substituted, preferably with one or two C 1-4 Alkyl, C 1-4 Alkoxy substitution; R1, R2 and R3 are the same or different and are independently selected from H, C 1-8 Alkyl, C 1-8 Alkoxy; R1 is connected to a carbon atom on the A ring; B - represents an anion, such as OH - .

2. The polymer according to claim 1, wherein R1, R2 and R3 are the same or different and are independently selected from H, C 1-4 Alkyl, C 1-4 Alkoxy; Preferably, R1, R2 and R3 are the same and are selected from H, methyl, ethyl, propyl, butyl, methoxy or ethoxy; Preferably, the nitrogen atom on A is substituted by two groups, for example, any two groups selected from methyl, ethyl, propyl, butyl, methoxy or ethoxy; And / or, A represents a saturated or unsaturated five-membered ring containing one nitrogen atom, a five-membered ring containing two nitrogen atoms, or a six-membered ring containing one nitrogen atom.

3. The polymer according to claim 1, wherein The molecular weight of the polymer is 20,000 to 100,000 g / mol.

4. The polymer according to any one of claims 1 to 3, wherein The polymer has a structure as shown in Formula I-1: R4 and R5 are the same or different and are independently selected from H, C 1-8 Alkyl, C 1-8 Alkoxy, preferably C 1-4 Alkyl, C 1-4 Alkoxy; Preferably, the polymer has a structure as shown in Formula I-2: 。 5. The method for preparing a polymer according to any one of claims 1 to 4, wherein: The preparation method comprises: reacting and soaking the polymer of formula D in an alkaline solution to obtain the polymer of formula I; wherein X represents a halogen, such as F, Cl, Br or I.

6. The preparation method according to claim 5, wherein: The preparation of the polymer of formula D comprises: reacting the polymer of formula C with a haloalkyl R5X in NMP or in a system further adding DMSO to obtain the polymer of formula D; Preferably, the alkyl halide R5X is methyl iodide; Preferably, the molar ratio of the alkyl halide R5X to the polymer structural unit of formula C is (2-5):1; Preferably, the polymer of formula C is first added to NMP until it can no longer be dissolved, and then DMSO is added thereto.

7. The preparation method according to claim 6, wherein: The preparation of the polymer of formula C comprises: reacting a compound of formula A and a compound of formula B in a system of trifluoroacetic acid, trifluoromethanesulfonic acid (TFSA) and dichloromethane to obtain a polymer of formula C; Preferably, the compound of formula A is selected from 8. Use of the polymer according to any one of claims 1 to 4 as an anion exchange membrane.

9. An anion exchange membrane prepared from the polymer according to any one of claims 1 to 4.

10. Use of the polymer according to any one of claims 1 to 4 or the anion exchange membrane according to claim 9 in hydrogen production by water electrolysis or CO2 conversion.