Preparation method of castor oil-based waterborne polyurethane ionic gel

By introducing PET degradation products and ionic liquids into castor oil-based water-based polyurethane, a stable castor oil-based water-based polyurethane ionic gel was prepared, which solved the problem of volatility of hydrogel solvents, improved its mechanical properties and electrical conductivity. in sensor equipment.

CN118909225APending Publication Date: 2024-11-08WEINAN KELINLE ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410988572.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The solvent of the hydrogel is easily volatile, causing it to be unstable and affecting its application in sensing equipment.

Method used

Using castor oil as raw material, polyurethane prepolymers are synthesized by introducing PET degradation products GOPs and isophorone diisocyanate, and mixed with 1-ethyl-3-methylimidazolodicyandiamide [EMIM][DCA] ionic liquid , prepare castor oil-based aqueous polyurethane ionic gel to form stable ionic conductive channels.

Benefits of technology

It improves the mechanical properties and tensile strength of castor oil-based water-based polyurethane, enhances the conductivity and stability of ionic gels, and provides a preparation method for bio-based ionic gels, suitable for flexible sensing equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909225A_ABST
    Figure CN118909225A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of castor oil-based waterborne polyurethane ionic gel, and relates to the technical field of polyurethane materials.The preparation method comprises the following steps that S1, castor oil serves as a raw material, GOPs replaces part of castor oil to serve as polyhydric alcohol, and blending and stirring are conducted for 24 h till swelling; s2, active oligomer polyol prepared from castor oil and GOPs is used as a raw material and reacts with isophorone diisocyanate (IPDI), a polyurethane prepolymer is synthesized, and the ratio of-NCO isocyanate to-OH polyol is 1.7. A benzene ring structure of a PET degradation product GOPs is introduced into a polyurethane structure, the ratio of a soft segment to a hard segment is adjusted to obtain a castor oil-based waterborne polyurethane material with excellent mechanical properties, then the castor oil-based waterborne polyurethane material is mixed and stirred with an ionic liquid to prepare the castor oil-based waterborne polyurethane ionic gel, and the castor oil-based waterborne polyurethane ionic gel is used as a raw material. The conductivity of the ionic gel is enhanced, meanwhile, the good tensile strength of the ionic gel is guaranteed, the bio-based WPU is combined with the ionic gel, and reference significance is provided for preparation of the bio-based ionic gel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane materials, in particular to a method for preparing castor oil-based waterborne polyurethane ion gel. Background Art

[0002] As the country attaches great importance to environmental protection, solvent-based polyurethanes containing volatile organic compounds (VOCs) are gradually replaced by waterborne polyurethanes (WPU). The raw materials for the synthesis of WPU include polyols, diisocyanates, emulsifiers and chain extenders, most of which are extracted from non-renewable resources-petroleum. In the current context of the depletion of petroleum resources, people have begun to pay attention to biomass resources. Biomass raw materials come from a wide range of sources, including cellulose, lignin and vegetable oils. Among them, vegetable oils are considered to be the most promising alternative to polyols in the synthesis of WPU because of their renewable, easy to obtain and low cost. Among them, castor oil is a natural vegetable oil polyol containing multiple hydroxyl groups, which can be directly synthesized into polyurethane without modification. However, the flexible long chain of castor oil fatty acids and the relatively low OH value of polyols cause the resulting WPU film to suffer certain limitations in mechanical and thermal properties, such as relatively low tensile strength and glass transition temperature. Adjusting the ratio between soft and hard segments, enhancing intermolecular interactions, adding nanomaterials, fiber materials, or increasing crosslinking density can improve the performance of castor oil-based WPU. Introducing a rigid structure into polyurethane can improve its mechanical properties. Introducing PET degradation product GOPs into the polyurethane structure can improve the mechanical properties of castor oil-based waterborne polyurethane.

[0003] Aqueous polyurethane emulsions can be prepared into gels for use in sensing devices. Traditional hydrogels are a type of 3D cross-linked hydrated polymer network that uses ions as charge carriers and converts subtle changes into detectable electrical signals by monitoring external stimuli such as pressure, strain, temperature or humidity. They have great potential in sensor applications, but the solvents of hydrogels are volatile, making them unstable. The structure of ion gels is similar to that of hydrogels. Ionic conductors based on ionic liquids (ILs) have received great attention as a new generation of flexible sensing devices due to their non-volatility, excellent thermal stability, better antifreeze performance and ionic conductivity.

[0004] Therefore, a method for preparing castor oil-based waterborne polyurethane ion gel is proposed. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing a castor oil-based waterborne polyurethane ion gel, which solves the problem that the solvent of the hydrogel is volatile, resulting in its instability.

[0006] To achieve the above object, the present invention is implemented by the following technical scheme: A method for preparing a castor oil-based waterborne polyurethane ion gel comprises the following steps:

[0007] S1, using castor oil as raw material, GOPs replace part of castor oil as polyol, and mixing and stirring for 24 hours until swelling;

[0008] S2, using active oligomer polyol prepared from castor oil and GOPs as raw materials, reacting with isophorone diisocyanate (IPDI) to synthesize polyurethane prepolymer, wherein -NCO isocyanate: -OH polyol = 1.7;

[0009] S3, using 1,4-butanediol as a small molecule chain extender, adding triethylamine to form a salt, and emulsifying with deionized water at high speed shearing to obtain a castor oil-based waterborne polyurethane (WPU) emulsion;

[0010] S4. Mixing castor oil-based waterborne polyurethane with ionic liquid to prepare ionic gel.

[0011] Preferably, the step S1 is specifically:

[0012] Step S1.1, degrading waste PET plastic sheets with dipropylene glycol and neopentyl glycol to prepare degradation products GOPs;

[0013] Step S1.2, weigh 0-5 parts of GOPs and 23-46 parts of castor oil, mix them, adjust the speed to 300 r / min under magnetic stirring, and stir for 24 hours to obtain active oligomer polyol (GCO).

[0014] Preferably, the step S2 is specifically:

[0015] Step S2.1, placing the active oligomer polyol (GCO) in a vacuum drying oven, adjusting the vacuum degree to 0.08 MPa, setting the temperature to 120° C., and drying for 12 h;

[0016] Step S2.2: Weigh 13 parts of isophorone diisocyanate and place them together with the oligomer polyol in a three-necked flask, and react in a water bath.

[0017] Preferably, in step S2.2, the rotation speed is adjusted to 250 r / min, the reaction is carried out in a water bath at 80°C for 10 min, 2-3 drops of tetramethylguanidine are added as a catalyst and the reaction is carried out for 5 min, the rotation speed is adjusted to 300 r / min, 13 parts of dihydroxymethylpropionic acid are weighed, the reaction is carried out for 1 h, and an appropriate amount of acetone is added during the reaction to adjust the viscosity of the system.

[0018] Preferably, the step S3 is specifically:

[0019] Step S3.1, cool to 40°C, weigh 3 parts of BDO, add, and react at 400 r / min for 1 h;

[0020] Step S3.2, add 8 parts of TEA and react for 2 minutes;

[0021] Step S3.3, weigh 70 parts of deionized water and add twice;

[0022] Step S3.4, testing the acidity and alkalinity of the emulsion with pH test paper, and adjusting the pH value of the system to neutral with potassium hydroxide solution;

[0023] Step S3.5, pour the emulsion onto a polytetrafluoroethylene (PTFE) substrate, and evaporate the solvent at 60°C to form a film.

[0024] Preferably, when deionized water is added in step S3.3, the rotation speed is adjusted to 700 r / min and 900 r / min respectively, and emulsification is performed for 2 minutes to obtain a castor oil-based waterborne polyurethane (WPU) emulsion.

[0025] Preferably, the step S4 is specifically:

[0026] Step S4.1, weigh 30 parts of 1-ethyl-3-methylimidazole dicyandiamide [EMIM] [DCA] and dissolve them in 70 parts of water;

[0027] Step S4.2: Weigh 50-90 parts of castor oil-based WPU emulsion and 10-50 parts of [BMIM][DCA], mix them, stir them mechanically, and cast them on a polytetrafluoroethylene (PTFE) substrate.

[0028] Preferably, the step S4.2 is followed by evaporation of the solvent at 25° C. and 60% humidity to form an ion gel WPU / ILx (x is the mass ratio of IL:WPU).

[0029] Beneficial Effects

[0030] The present invention provides a method for preparing a castor oil-based waterborne polyurethane ion gel. Compared with the prior art, the method has the following beneficial effects:

[0031] (1) The method for preparing the castor oil-based waterborne polyurethane ion gel is to introduce the benzene ring structure of the PET degradation product GOPs into the polyurethane structure, adjust the ratio between the soft segment and the hard segment, obtain a castor oil-based waterborne polyurethane material with excellent mechanical properties, and then mix and stir the castor oil-based waterborne polyurethane material with an ionic liquid to prepare the castor oil-based waterborne polyurethane ion gel, while enhancing the conductivity of the ion gel and ensuring its good tensile strength, combining the bio-based WPU with the ion gel, and providing a reference for the preparation of the bio-based ion gel;

[0032] (2) The preparation method of the castor oil-based waterborne polyurethane ion gel, the solid degradation products of discarded PET bottles (GOPs) contain a rigid structure, which can improve the mechanical properties of the castor oil-based waterborne polyurethane. At the same time, the carboxylic acid structure is introduced into the WPU hard segment to imitate the ion transmission channel in the phospholipid bilayer of the cell membrane. The hydrogen bonding effect makes the hard segment domain regularly arranged to form an ion conductive channel;

[0033] (3) A method for preparing the castor oil-based waterborne polyurethane ion gel, using biomass material castor oil and waste PET degradation product GOPs as polyols, and isophorone diisocyanate to prepare waterborne polyurethane, introducing the rigid structure in GOPs into the polyurethane structure to improve the mechanical properties of the polyurethane film, and using the prepared castor oil-based waterborne polyurethane to mix with the ionic liquid 1-ethyl-3-methylimidazole dicyandiamide [EMIM] [DCA] to prepare the ion gel;

[0034] (4) The method for preparing the castor oil-based aqueous polyurethane ion gel shows that the prepared aqueous polyurethane ion gel presents a uniform nanoparticle microstructure, proving that a uniform ion gel is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of the connection steps of the present invention;

[0036] Figure 2 This is a 100nm transmission electron microscope image of the castor oil-based waterborne polyurethane ion gel of the present invention;

[0037] Figure 3 This is a 200nm transmission electron microscope image of the castor oil-based waterborne polyurethane ion gel of the present invention;

[0038] Figure 4 This is a 0.5 μm transmission electron microscope image of the castor oil-based waterborne polyurethane ion gel of the present invention. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] See also Figure 1 - Figure 4 The present invention provides three technical solutions, which specifically include the following embodiments:

[0041] Embodiment 1:

[0042] A method for preparing a castor oil-based waterborne polyurethane ion gel comprises the following steps:

[0043] S1, using castor oil as raw material, GOPs replace part of castor oil as polyol, and mixing and stirring for 24 hours until swelling;

[0044] Step S1.1, degrading waste PET plastic sheets with dipropylene glycol and neopentyl glycol to prepare degradation products GOPs;

[0045] Step S1.2, weighing 1 part of GOPs and 42 parts of castor oil, mixing them, adjusting the speed to 300 r / min and stirring for 24 hours under magnetic stirring, to obtain active oligomer polyol (GCO);

[0046] S2, using active oligomer polyol prepared from castor oil and GOPs as raw materials, reacting with isophorone diisocyanate (IPDI) to synthesize polyurethane prepolymer, wherein -NCO isocyanate: -OH polyol = 1.7;

[0047] Step S2.1, placing the active oligomer polyol (GCO) in a vacuum drying oven, adjusting the vacuum degree to 0.08 MPa, setting the temperature to 120° C., and drying for 12 h;

[0048] Step S2.2, weigh 13 parts of isophorone diisocyanate, place it in a three-necked flask together with the oligomer polyol, and react in a water bath environment. Adjust the speed to 250r / min, react in a water bath at 80℃ for 10min; add 2 drops of tetramethylguanidine as a catalyst and react for 5min; adjust the speed to 300r / min, weigh 13 parts of dimethylol propionic acid, react for 1h, and add appropriate amount of acetone to adjust the viscosity of the system;

[0049] S3, using 1,4-butanediol as a small molecule chain extender, adding triethylamine to form a salt, and emulsifying with deionized water at high speed shearing to obtain a castor oil-based waterborne polyurethane (WPU) emulsion;

[0050] Step S3.1, cool to 40°C, weigh 3 parts of BDO, add, and react at 400 r / min for 1 h;

[0051] Step S3.2, add 8 parts of TEA and react for 2 minutes;

[0052] Step S3.3, weigh 70 parts of deionized water, add twice, adjust the speed to 700 r / min and 900 r / min respectively, emulsify for 2 minutes, and obtain castor oil-based waterborne polyurethane (WPU) emulsion,

[0053] Step S3.4, testing the acidity and alkalinity of the emulsion with pH test paper, and adjusting the pH value of the system to neutral with potassium hydroxide solution;

[0054] Step S3.5, pour the emulsion onto a polytetrafluoroethylene (PTFE) substrate, and evaporate the solvent at 60°C to form a film.

[0055] S4. Mixing castor oil-based waterborne polyurethane with ionic liquid to prepare ionic gel.

[0056] Step S4.1, weigh 30 parts of 1-ethyl-3-methylimidazole dicyandiamide [EMIM] [DCA] and dissolve them in 70 parts of water.

[0057] Step S4.2, weigh 50 parts of castor oil-based WPU emulsion and 90 parts of [BMIM][DCA], mix them and stir them mechanically, and cast them on a polytetrafluoroethylene (PTFE) substrate. The process is followed by solvent evaporation at 25°C and 60% humidity to form an ion gel WPU / ILx (x is the mass ratio of IL:WPU).

[0058] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0059] Embodiment 2:

[0060] A method for preparing a castor oil-based waterborne polyurethane ion gel comprises the following steps:

[0061] S1, using castor oil as raw material, GOPs replace part of castor oil as polyol, and mixing and stirring for 24 hours until swelling;

[0062] Step S1.1, degrading waste PET plastic sheets with dipropylene glycol and neopentyl glycol to prepare degradation products GOPs;

[0063] Step S1.2, weigh 2 parts of GOPs and 37 parts of castor oil, mix them, adjust the speed to 300 r / min under magnetic stirring, and stir for 24 hours to obtain active oligomer polyol (GCO).

[0064] S2, using active oligomer polyol prepared from castor oil and GOPs as raw materials, reacting with isophorone diisocyanate (IPDI) to synthesize polyurethane prepolymer, wherein -NCO isocyanate: -OH polyol = 1.7;

[0065] Step S2.1, placing the active oligomer polyol (GCO) in a vacuum drying oven, adjusting the vacuum degree to 0.08 MPa, setting the temperature to 120° C., and drying for 12 h;

[0066] Step S2.2, weigh 13 parts of isophorone diisocyanate, place them together with the oligomer polyol in a three-necked flask, react in a water bath environment, adjust the speed to 250r / min, react in a water bath at 80°C for 10min, add 3 drops of tetramethylguanidine as a catalyst and react for 5min, adjust the speed to 300r / min, weigh 13 parts of dimethylol propionic acid, react for 1h, and add an appropriate amount of acetone to adjust the viscosity of the system;

[0067] S3, using 1,4-butanediol as a small molecule chain extender, adding triethylamine to form a salt, and emulsifying with deionized water at high speed shearing to obtain a castor oil-based waterborne polyurethane (WPU) emulsion;

[0068] Step S3.1, cool to 40°C, weigh 3 parts of BDO, add, and react at 400 r / min for 1 h;

[0069] Step S3.2, add 8 parts of TEA and react for 2 minutes,

[0070] Step S3.3, weigh 70 parts of deionized water, add twice, adjust the speed to 700 r / min and 900 r / min respectively, emulsify for 2 minutes, and obtain castor oil-based waterborne polyurethane (WPU) emulsion,

[0071] Step S3.4: Use pH test paper to test the acidity and alkalinity of the emulsion, and use potassium hydroxide solution to adjust the pH value of the system to neutral.

[0072] Step S3.5, pour the emulsion onto a polytetrafluoroethylene (PTFE) substrate, and evaporate the solvent at 60°C to form a film.

[0073] S4. Mixing castor oil-based waterborne polyurethane with ionic liquid to prepare ionic gel.

[0074] Step S4.1, weigh 30 parts of 1-ethyl-3-methylimidazole dicyandiamide [EMIM] [DCA] and dissolve them in 70 parts of water;

[0075] Step S4.2, weigh 70 parts of castor oil-based WPU emulsion and 30 parts of [BMIM][DCA], mix them and stir them mechanically, and cast them on a polytetrafluoroethylene (PTFE) substrate. The process is followed by solvent evaporation at 25°C and 60% humidity to form an ion gel WPU / ILx (x is the mass ratio of IL:WPU).

[0076] Embodiment three:

[0077] A method for preparing a castor oil-based waterborne polyurethane ion gel comprises the following steps:

[0078] S1, using castor oil as raw material, GOPs replace part of castor oil as polyol, and mixing and stirring for 24 hours until swelling;

[0079] Step S1.1, degrading waste PET plastic sheets with dipropylene glycol and neopentyl glycol to prepare degradation products GOPs;

[0080] Step S1.2, weighing 3 parts of GOPs and 33 parts of castor oil, mixing them, adjusting the speed to 300 r / min under magnetic stirring for 24 hours, to obtain active oligomer polyol (GCO);

[0081] S2, using active oligomer polyol prepared from castor oil and GOPs as raw materials, reacting with isophorone diisocyanate (IPDI) to synthesize polyurethane prepolymer, wherein -NCO isocyanate: -OH polyol = 1.7;

[0082] Step S2.1, placing the active oligomer polyol (GCO) in a vacuum drying oven, adjusting the vacuum degree to 0.08 MPa, setting the temperature to 120° C., and drying for 12 h;

[0083] Step S2.2, weigh 13 parts of isophorone diisocyanate, place them together with the oligomer polyol in a three-necked flask, react in a water bath environment, adjust the speed to 250r / min, react in a water bath at 80°C for 10min, add 3 drops of tetramethylguanidine as a catalyst and react for 5min, adjust the speed to 300r / min, weigh 13 parts of dimethylol propionic acid, react for 1h, and add an appropriate amount of acetone to adjust the viscosity of the system;

[0084] S3, using 1,4-butanediol as a small molecule chain extender, adding triethylamine to form a salt, and emulsifying with deionized water at high speed shearing to obtain a castor oil-based waterborne polyurethane (WPU) emulsion;

[0085] Step S3.1, cool to 40°C, weigh 3 parts of BDO, add, and react at 400 r / min for 1 h;

[0086] Step S3.2, add 8 parts of TEA and react for 2 minutes,

[0087] Step S3.3, weigh 70 parts of deionized water, add twice, adjust the speed to 700 r / min and 900 r / min respectively, emulsify for 2 minutes, and obtain castor oil-based waterborne polyurethane (WPU) emulsion,

[0088] Step S3.4, testing the acidity and alkalinity of the emulsion with pH test paper, and adjusting the pH value of the system to neutral with potassium hydroxide solution;

[0089] Step S3.5, pour the emulsion onto a polytetrafluoroethylene (PTFE) substrate, and evaporate the solvent at 60°C to form a film.

[0090] S4. Mixing castor oil-based waterborne polyurethane with ionic liquid to prepare ionic gel.

[0091] Step S4.1, weigh 30 parts of 1-ethyl-3-methylimidazole dicyandiamide [EMIM] [DCA] and dissolve them in 70 parts of water;

[0092] Step S4.2, weigh 90 parts of castor oil-based WPU emulsion and 10 parts of [BMIM][DCA], mix them for mechanical stirring, and cast them on a polytetrafluoroethylene (PTFE) substrate. The process is followed by solvent evaporation at 25°C and 60% humidity to form an ion gel WPU / ILx (x is the mass ratio of IL:WPU).

[0093] The mechanism of action of the method of the present invention is:

[0094] The solid degradation products (GOPs) of discarded PET bottles contain rigid structures, which can improve the mechanical properties of castor oil-based waterborne polyurethane. At the same time, the carboxylic acid structure is introduced into the hard segment of WPU to imitate the ion transport channel in the phospholipid bilayer of the cell membrane. The hydrogen bonding effect makes the hard segment domains arranged regularly to form an ion conductive channel.

[0095] The benzene ring structure of PET degradation product GOPs was introduced into the polyurethane structure, and the ratio between the soft segment and the hard segment was adjusted to obtain a castor oil-based waterborne polyurethane material with excellent mechanical properties. Then it was mixed and stirred with ionic liquid to prepare castor oil-based waterborne polyurethane ion gel, which enhanced the conductivity of the ion gel while ensuring its good tensile strength. The combination of bio-based WPU and ion gel provides a reference for the preparation of bio-based ion gel.

[0096] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the application should be included in the protection scope of the present application.

Claims

1. A method for preparing a castor oil-based waterborne polyurethane ion gel, Features: The following steps are involved: S1, using castor oil as raw material, GOPs replace part of castor oil as polyol, and mixing and stirring for 24 hours until swelling; S2, using active oligomer polyol prepared from castor oil and GOPs as raw materials, reacting with isophorone diisocyanate (IPDI) to synthesize polyurethane prepolymer, wherein -NCO isocyanate: -OH polyol = 1.7; S3, using 1,4-butanediol as a small molecule chain extender, adding triethylamine to form a salt, and emulsifying with deionized water at high speed shearing to obtain a castor oil-based waterborne polyurethane (WPU) emulsion; S4. Mixing castor oil-based waterborne polyurethane with ionic liquid to prepare ionic gel.

2. A method for preparing a castor oil-based waterborne polyurethane ion gel according to claim 1, Features: The step S1 is specifically: Step S1.1, degrading waste PET plastic sheets with dipropylene glycol and neopentyl glycol to prepare degradation products GOPs; Step S1.2, weigh 0-5 parts of GOPs and 23-46 parts of castor oil, mix them, adjust the speed to 300 r / min under magnetic stirring, and stir for 24 hours to obtain active oligomer polyol (GCO).

3. A method for preparing a castor oil-based waterborne polyurethane ion gel according to claim 1, Features: The step S2 is specifically: Step S2.1, placing the active oligomer polyol (GCO) in a vacuum drying oven, adjusting the vacuum degree to 0.08 MPa, setting the temperature to 120° C., and drying for 12 h; Step S2.2: Weigh 13 parts of isophorone diisocyanate and place them together with the oligomer polyol in a three-necked flask, and react in a water bath.

4. A method for preparing a castor oil-based waterborne polyurethane ion gel according to claim 3, Features: In step S2.2, the rotation speed is adjusted to 250 r / min, the reaction is carried out in a water bath at 80° C. for 10 min, 2-3 drops of tetramethylguanidine are added as a catalyst and the reaction is carried out for 5 min, the rotation speed is adjusted to 300 r / min, 13 parts of dimethylolpropionic acid are weighed, and the reaction is carried out for 1 h, during which an appropriate amount of acetone is added to adjust the viscosity of the system.

5. A method for preparing a castor oil-based waterborne polyurethane ion gel according to claim 1, Features: The step S3 is specifically: Step S3.1, cool to 40°C, weigh 3 parts of BDO, add, and react at 400 r / min for 1 h; Step S3.2, add 8 parts of TEA and react for 2 minutes; Step S3.3, weigh 70 parts of deionized water and add twice; Step S3.4, testing the acidity and alkalinity of the emulsion with pH test paper, and adjusting the pH value of the system to neutral with potassium hydroxide solution; Step S3.5, pour the emulsion onto a polytetrafluoroethylene (PTFE) substrate, and evaporate the solvent at 60°C to form a film.

6. A method for preparing a castor oil-based waterborne polyurethane ion gel according to claim 5, Features: When adding deionized water in step S3.3, the rotation speed is adjusted to 700 r / min and 900 r / min respectively, and emulsification is performed for 2 minutes to obtain a castor oil-based waterborne polyurethane (WPU) emulsion.

7. A method for preparing a castor oil-based waterborne polyurethane ion gel according to claim 1, Features: The step S4 is specifically: Step S4.1, weigh 30 parts of 1-ethyl-3-methylimidazole dicyandiamide [EMIM] [DCA] and dissolve them in 70 parts of water; Step S4.2: Weigh 50-90 parts of castor oil-based WPU emulsion and 10-50 parts of [BMIM][DCA], mix them, stir them mechanically, and cast them on a polytetrafluoroethylene (PTFE) substrate.

8. A method for preparing a castor oil-based waterborne polyurethane ion gel according to claim 7, Features: The step S4.2 is followed by evaporation of the solvent at 25°C and 60% humidity to form an ion gel WPU / ILx (x is the mass ratio of IL:WPU).