Phenolic group-containing amine adduct and preparation method thereof

By introducing phenol hydroxyl groups in the epoxy-amine addition reaction, combining amines and chain extenders, phenol-containing amine adducts are prepared, which solves the risk of formaldehyde carcinogenicity and process complexity, and achieves high efficiency and environmental protection Epoxy resin curing, suitable for a variety of curing agent types.

CN118909227AActive Publication Date: 2024-11-08JIANGSU FUQISEN NEW MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411087904.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Formaldehyde is commonly used as a coupling agent in existing epoxy resin curing agents, which has a risk of carcinogenicity, and the process is complicated, making it difficult to cure quickly in a high-humidity environment.

Method used

The phenol hydroxyl group is introduced into the curing agent through a simple epoxy-amine addition reaction, and the raw material amine and chain extender are combined to prepare the phenol amine adduct, which avoids formaldehyde. and curing properties are adjusted by capping agent.

Benefits of technology

It achieves efficient curing without formaldehyde residues, simplifies the process flow, improves the low-temperature curing performance and environmental protection, and is suitable for solvent-free, solvent-based and aqueous epoxy curing agents, meeting the needs of rapid curing and high-humidity environment construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a phenolic group-containing amine adduct and a preparation method thereof in the technical field of epoxy hardener preparation, and the preparation method comprises the following steps: 1) mixing an aminophenol compound, a solvent and a chain extender at 80-120 DEG C to react for 4-8 hours, then adding an end-capping reagent to mix to obtain an intermediate, and 2) dropwise adding the intermediate into a raw material amine, and reacting at 60-90 DEG C for 2-8 hours to obtain the phenolic group-containing amine adduct, according to the scheme, the amine curing agent with phenolic hydroxyl groups in the structure is obtained, compared with a phenolic amine technology based on Mannich reaction, toxic aldehyde ketone compounds are not needed, a complex dehydration process is also not needed, the synthesis process is simple and efficient, and the raw material conversion rate is high; as an epoxy resin curing agent, the product has the advantages of high curing speed, low-temperature curing, no oil surface whitening phenomenon in a high-humidity environment and the like, a water-based product can be prepared by selecting specific raw materials, and the application range is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy resin curing agents, and in particular to a phenolic amine adduct and a preparation method thereof. Background Art

[0002] Amines and their modifications are often used as curing agents for epoxy resins. However, whether it is epoxy resin-added amines or polyamides, they all have the problem of slow curing at low temperatures. In particular, in high humidity environments, amine compounds cannot react with epoxy in time, but instead absorb moisture and carbon dioxide and migrate to the surface, resulting in "oily surface" and "whitening" and other drawbacks. In order to solve the above problems, phenols are usually used as promoters. The principle is that phenolic hydroxyl groups are weakly acidic, and they combine with the more electronegative oxygen atoms in the epoxy group to promote the ring opening of the epoxy group and accelerate the reaction rate; and phenolic hydroxyl groups can undergo a reversible weak salt-forming reaction with amines, inhibiting the salt formation of amines and carbon dioxide, and not interfering with the chemical reaction stoichiometry of the epoxy group and the active hydrogen of the amine.

[0003] In order to use phenolic hydroxyl groups in epoxy resin systems, one method is to directly add phenolic compounds to epoxy resins or curing agents. Small molecular phenols such as phenol, o-cresol and salicylic acid have obvious crystallinity and poor compatibility with resins; long-chain alkylphenols represented by nonylphenol are gradually restricted or even banned due to their reproductive toxicity and high toxicity to aquatic organisms; although styrenated phenol has excellent comprehensive properties, it does not participate in the cross-linking and curing reaction itself, and a large amount will significantly reduce the cross-linking density of the cured product, so the effect is limited. Another method is to introduce phenolic hydroxyl groups into the structure of amines through chemical synthesis. The typical representative is phenolic amine, which is obtained by Mannich condensation reaction of phenol (phenol, cardanol, etc.), aldehydes (mainly formaldehyde), and polyamines. It has been widely used in the field of epoxy resin curing agents.

[0004] The phenolic hydroxyl content in the phenalkamine structure is high, the reaction speed is fast when curing with epoxy resin, the cross-linking density is high, and it has good low-temperature curing properties and excellent physical and chemical properties. However, the technical route for preparing phenolic amines by the Mannich reaction has inevitable defects: phenolic amines generally use formaldehyde as a coupling agent for phenol and amine. It is well known that formaldehyde is a Class 1 carcinogen, which has chronic and long-term harm to the human body; whether formaldehyde aqueous solution or polyformaldehyde is used, formaldehyde residue and volatilization exist in the production process and the finished product, posing a threat to the health of production personnel and users; in order to remove the hazards of formaldehyde, some inventions use other coupling agents based on the Mannich reaction, such as CN201610738722.6, a Mannich base epoxy resin curing agent, which uses benzaldehyde to react with cardanol and polyamines, dehydrates and cools after the reaction, and then adds isooctanoic acid and stirs to obtain the product; CN202110490672.5 mentions a preparation method of an aldehyde-free water-based cardanol ketone amine epoxy curing agent, which uses ketones instead of aldehydes for the Mannich reaction. According to the mechanism of the Mannich reaction, if a substituted aldehyde (benzaldehyde) or ketone is used, the reaction rate and raw material conversion rate will be greatly reduced because the steric hindrance effect is much greater than that of formaldehyde. Therefore, although the technical route of the above invention is theoretically feasible, it lacks practical application value. A large number of small molecular aldehyde and ketone compounds remain in the system, which are also irritating and toxic. On the other hand, the Mannich reaction is a condensation reaction, and a dehydration operation must be performed to increase the conversion rate, and the process is complicated. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a phenolic amine adduct and a preparation method thereof, which solves the risk of formaldehyde commonly used in the existing phenolic amine technology and promotes the technical development of solvent-free, solvent-based and water-based epoxy curing agents.

[0006] The object of the present invention is achieved in this way: a phenolic amine adduct is prepared by comprising the following raw materials in parts by weight: 10-40 parts of raw material amine, 10-30 parts of aminophenol, 20-50 parts of chain extender, and 10-35 parts of end-capping agent.

[0007] Furthermore, the raw material amine includes one or more of aliphatic amine, alicyclic amine, aromatic amine and polyether amine.

[0008] Further, the fatty amine comprises one or more of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, diethylenetriamine, triethylenetetramine and N,N-bis(3-aminopropyl)ethylenediamine; The alicyclic amine comprises one or more of menthanediamine, isophoronediamine, 1,3-cyclohexanedimethylamine, methylcyclohexanediamine and 4,4-diaminodicyclohexylmethane; The aromatic amine is 1,3-m-phenylenediamine; The polyetheramine is selected from one or more of the trade names D230, D400, D2000 and ED2003.

[0009] Furthermore, the aminophenol comprises one or more of 3-aminophenol, p-aminophenol, p-aminophenol, o-amino-p-tert-butylphenol, 2-aminoresorcinol, and 2-amino-4-cyclohexylphenol.

[0010] Furthermore, the chain extender is selected from one or more of bisphenol A epoxy resin with an epoxy equivalent of 100 to 600 g / eq, ethylene glycol diglycidyl ether with an epoxy equivalent of 100 to 600 g / eq, polypropylene glycol diglycidyl ether with an epoxy equivalent of 200 to 800 g / eq, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, dipropylene glycol diglycidyl ether and dimer acid diglycidyl ester.

[0011] Furthermore, the end-capping agent is selected from one or more of butyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether, C12-14 alkyl glycidyl ether, neodecanoic acid glycidyl ester, and cardanol glycidyl ether.

[0012] A method for preparing a phenolic amine adduct comprises the following steps: Step 1) aminophenol and a chain extender are mixed, and the mixture is heated to a certain temperature to react to obtain an intermediate, and then a capping agent is added and mixed to obtain a dropwise solution; Step 2) adding the dropwise addition liquid to the heated raw material amine within a set time to react and keep the temperature, and obtaining a phenolic amine adduct after the temperature is kept.

[0013] Furthermore, the specific process of the reaction in step 1) is: heating to 80-120°C and keeping warm for 4-8h; The specific process of the reaction in step 2) is: the temperature of the bottom liquid of the kettle is raised to 60-90°C, the temperature of the dropwise liquid is maintained at 20-40°C, the dropwise addition is performed for 1-4 hours, and after the dropwise addition is completed, the temperature is maintained at 60-90°C for 1-4 hours to obtain a phenolic amine adduct.

[0014] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention uses amino-containing phenolic compounds (aminophenols) to introduce phenolic hydroxyl groups into the chemical structure of the curing agent based on a simple and mature epoxy-amine addition reaction. There are no volatile carcinogens in the raw materials and products. The raw material conversion rate is high during the reaction, there is almost no side reaction, the process is simple and easy to produce, and the shortcomings of existing phenolic amine technology, such as health risks and complex processes, can be solved. (2) The present invention can conveniently and flexibly adjust the curing speed, hardness, flexibility, hydrophilicity and other performance indicators by selecting the raw material amine, chain extender and end-capping agent. Therefore, based on the same process, both the curing agent for solvent-free or solvent-based system and the water-based curing agent can be prepared; (3) The phenolic amine adduct obtained by the present invention can be directly used as a single curing agent, or can be mixed with other amine curing agents to improve its low-temperature curing performance and other properties, and has a wide range of uses. DETAILED DESCRIPTION

[0015] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0016] Example 1 A method for preparing a phenolic amine adduct A comprises the following steps: (1) Add 10 parts by weight of D230 polyetheramine, 5 parts by weight of ethylenediamine and 18 parts by weight of isophoronediamine into a reaction kettle, mix well and heat to 65°C to prepare the bottom liquid; (2) Add 9 parts by weight of 3-aminophenol and 25 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 to a dropping tank, mix and heat to 100°C and keep warm for 4 hours, then add 18 parts by weight of butyl glycidyl ether and 15 parts by weight of phenyl glycidyl ether, mix and cool to 30°C, and drip into the bottom liquid of the kettle for 3 hours, maintaining the temperature of the material in the kettle at 65°C. After the dripping is completed, the temperature of the material in the kettle is raised to 80°C and kept warm for 3 hours to obtain a phenolic amine adduct A with an active hydrogen equivalent of 131 g / eq. (3) Take 41 parts by weight of phenolic amine adduct A and 59 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container. Take a small amount and use a 100 μm wire rod to make a film on a tinplate. Put it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours and observe the appearance of the coating; divide the remaining mixed liquid into two parts, put them in an environment of 25°C and 5°C respectively, and record the gel time.

[0017] Example 2 A method for preparing a phenolic amine adduct B comprises the following steps: (1) Add 20 parts by weight of D400 polyetheramine and 10 parts by weight of diethylenetriamine into a reaction kettle, mix well, and heat to 70°C to prepare the bottom liquid for later use; (2) Add 10 parts by weight of p-aminophenol, 28 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq, and 17 parts by weight of polypropylene glycol diglycidyl ether with an epoxy equivalent of 300 g / eq into a dropping tank, mix, heat to 100°C, and keep warm for 4 hours. Then add 15 parts by weight of o-cresol glycidyl ether, mix, cool to 30°C, and drop it into the bottom liquid of the kettle for 3 hours, maintaining the temperature of the material in the kettle at 70°C. After the dropwise addition, raise the temperature of the material in the kettle to 80°C and keep warm for 3 hours to obtain phenolic amine adduct B with an active hydrogen equivalent of 173 g / eq. (3) Take 48 parts by weight of phenolic amine adduct B and 52 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container. Take a small amount and use a 100 μm wire rod to make a film on a tinplate. Put it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours and observe the appearance of the coating; divide the remaining mixed liquid into two parts, put them in an environment of 25°C and 5°C respectively, and record the gel time.

[0018] Example 3 A method for preparing a phenolic amine adduct C comprises the following steps: (1) Add 17 parts by weight of isophorone diamine and 10 parts by weight of diethylene triamine into a reaction kettle, mix well, and heat to 70°C to prepare the bottom liquid for later use; (2) Add 15 parts by weight of p-aminophenol and 33 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq to a dropping tank, heat to 120°C and keep warm for 4 hours, then add 25 parts by weight of C12-14 alkyl glycidyl ether, cool to 30°C, and drop into the bottom liquid for 3 hours, maintaining the temperature of the material in the kettle at 70°C. After the dropwise addition, raise the temperature of the material in the kettle to 80°C and keep warm for 3 hours to obtain a phenolic amine adduct C with an active hydrogen equivalent of 133 g / eq. (3) Take 41 parts by weight of phenolic amine adduct C and 59 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container. Take a small amount and use a 100 μm wire rod to make a film on a tinplate. Put it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours and observe the appearance of the coating; divide the remaining mixed liquid into two parts, put them in an environment of 25°C and 5°C respectively, and record the gel time.

[0019] Example 4 A method for preparing a phenolic amine adduct D comprises the following steps: (1) Add 20 parts by weight of D2000 polyetheramine and 18 parts by weight of diethylenetriamine into a reaction kettle, mix well, and heat to 70°C to prepare the bottom liquid for later use; (2) Add 14 parts by weight of o-amino-p-tert-butylphenol and 32 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq to a dropping tank, mix, heat to 120°C and keep warm for 4 hours, then add 16 parts by weight of phenyl glycidyl ether, mix, cool to 30°C, and drop it into the bottom liquid of the kettle for 3 hours, maintaining the temperature of the material in the kettle at 70°C. After the dropwise addition, raise the temperature of the material in the kettle to 80°C and keep warm for 3 hours to obtain a phenolic amine adduct D with an active hydrogen equivalent of 123 g / eq. (3) Take 39 parts by weight of phenolic amine adduct D and 61 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container. Take a small amount and use a 100 μm wire rod to make a film on a tinplate. Put it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours and observe the appearance of the coating; divide the remaining mixed liquid into two parts, put them in an environment of 25°C and 5°C respectively, and record the gel time.

[0020] Example 5 A method for preparing a phenolic amine adduct E comprises the following steps: (1) Add 18 parts by weight of 1,6-hexanediamine and 4 parts by weight of diethylenetriamine into a reaction kettle, mix well, and heat to 60° C. to prepare the bottom liquid for later use; (2) Add 16 parts by weight of 2-aminoresorcinol, 30 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq, and 20 parts by weight of polyethylene glycol diglycidyl ether with an epoxy equivalent of 280 g / eq into a dropping tank, heat to 120°C and keep warm for 4 hours, then add 12 parts by weight of C12-14 alkyl glycidyl ether, cool to 30°C, and drip into the bottom liquid of the kettle for 3 hours, maintaining the temperature of the material in the kettle at 60°C. After the dripping is completed, the temperature of the material in the kettle is raised to 80°C and kept warm for 3 hours to obtain a phenolic amine adduct E with an active hydrogen equivalent of 120 g / eq. (3) Take 39 parts by weight of phenolic amine adduct E and 61 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container. Take a small amount and use a 100 μm wire rod to make a film on a tinplate. Put it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours and observe the appearance of the coating; divide the remaining mixed liquid into two parts, put them in an environment of 25°C and 5°C respectively, and record the gel time.

[0021] Example 6 A method for preparing a phenolic amine adduct F comprises the following steps: (1) Add 12 parts by weight of D400 polyetheramine and 20 parts by weight of isophorone diamine into a reaction kettle, mix well, and heat to 70°C to prepare the bottom liquid for later use; (2) Add 19 parts by weight of 2-amino-4-cyclohexylphenol, 22 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq, and 12 parts by weight of polyethylene glycol diglycidyl ether with an epoxy equivalent of 280 g / eq to a dropping tank, heat to 120°C and keep warm for 4 hours, then add 15 parts by weight of phenyl glycidyl ether, cool to 30°C, and drop it to the bottom liquid of the kettle for 3 hours, maintaining the temperature of the material in the kettle at 60°C. After the dropwise addition is completed, the temperature of the material in the kettle is raised to 80°C and kept warm for 3 hours to obtain a phenolic amine adduct F with an active hydrogen equivalent of 181 g / eq. (3) Take 49 parts by weight of phenolic amine adduct F and 51 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container. Take a small amount and use a 100 μm wire rod to make a film on a tinplate. Put it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours and observe the appearance of the coating; divide the remaining mixed liquid into two parts, place them in an environment of 25°C and 5°C respectively, and record the gel time.

[0022] Comparative Example 1 Take 34 parts by weight of a commercially available epoxy resin-added amine curing agent with an active hydrogen equivalent of 93 g / eq and 66 parts by weight of a bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container; take a small amount and use a 100 μm wire rod to make a film on a tinplate plate, place it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours, and observe the appearance of the coating; divide the remaining mixed liquid into two parts, place them in 25°C and 5°C environments respectively, and record the gel time.

[0023] Comparative Example 2 Take 33 parts by weight of a commercially available polyamide curing agent with an active hydrogen equivalent of 93 g / eq and 67 parts by weight of a bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container; take a small amount and use a 100 μm wire rod to make a film on a tinplate plate; place it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours and observe the appearance of the coating; divide the remaining mixed liquid into two parts, place them in 25°C and 5°C environments respectively, and record the gel time.

[0024] Comparative Example 3 Take 33 parts by weight of a commercially available phenolic amine curing agent with an active hydrogen equivalent of 95 g / eq and 67 parts by weight of a bisphenol A epoxy resin with an epoxy equivalent of 189 g / eq and mix them evenly in a container; take a small amount and use a 100 μm wire rod to make a film on a tinplate plate, place it in a constant temperature and humidity chamber at 5°C and 85% humidity to cure for 24 hours, and observe the appearance of the coating; divide the remaining mixed liquid into two parts, place them in 25°C and 5°C environments respectively, and record the gel time.

[0025] The present invention does not use formaldehyde and does not require complex processes such as dehydration, and is easy to mass produce. It can better meet the industry's needs for rapid curing, low-temperature curing, and construction in a high-humidity environment. By using an amino-containing phenolic compound (aminophenol), the phenolic hydroxyl group can be introduced into the chemical structure of the curing agent based on a simple and mature epoxy-amine addition reaction. The curing speed, hardness, flexibility, hydrophilicity and other performance indicators can be conveniently and flexibly adjusted through the screening of raw material amines, chain extenders and end-capping agents. The raw material conversion rate is high during the reaction, and there is almost no side reaction. The process is simple and easy to produce. It can solve the risk of formaldehyde commonly used in existing phenolic amine technology and has a driving effect on the technical development of solvent-free, solvent-based and water-based epoxy curing agents.

[0026] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

[0027] The performance tests described in the above examples and comparative examples include the gel time of the mixture of curing agent and epoxy resin at different temperatures, and the appearance of the coating in a low temperature and high humidity environment after film formation. The test results are shown in Table 1: Table 1: Curing properties of phenolic amine adducts

[0028] From the data in Table 1, it can be seen that when the phenolic amine adduct obtained by the present invention is used in combination with a standard liquid epoxy resin, its room temperature curing speed, low temperature curing performance and performance in a high humidity and low temperature environment are not inferior to or even better than commercially available phenalkamine curing agents, and are significantly better than addition amines and polyamides that are not modified with phenol. Therefore, the present invention can completely replace phenalkamine products using formaldehyde in terms of application performance, and is far superior to existing phenalkamine technologies in terms of environmental protection and production convenience.

[0029] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A phenolic amine adduct, It is characterized in that It is prepared from the following raw materials in parts by weight: 10-40 parts of raw material amine, 10-30 parts of aminophenol, 20-50 parts of chain extender, and 10-35 parts of end-capping agent.

2. A phenolic amine adduct according to claim 1, It is characterized in that The raw material amine comprises one or more of aliphatic amine, alicyclic amine, aromatic amine and polyether amine.

3. A phenolic amine adduct according to claim 2, It is characterized in that The fatty amine comprises one or more of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, diethylenetriamine, triethylenetetramine and N,N-bis(3-aminopropyl)ethylenediamine; The alicyclic amine comprises one or more of menthanediamine, isophoronediamine, 1,3-cyclohexanedimethylamine, methylcyclohexanediamine and 4,4-diaminodicyclohexylmethane; The aromatic amine is 1,3-m-phenylenediamine; The polyetheramine is selected from one or more of the trade names D230, D400, D2000 and ED2003.

4. A phenolic amine adduct according to any one of claims 1 to 3, It is characterized in that The aminophenol comprises one or more of 3-aminophenol, p-aminophenol, p-aminophenol, o-amino-p-tert-butylphenol, 2-aminoresorcinol, and 2-amino-4-cyclohexylphenol.

5. A phenolic amine adduct according to any one of claims 1 to 3, It is characterized in that The chain extender is selected from one or more of bisphenol A epoxy resin with an epoxy equivalent of 100 to 600 g / eq, ethylene glycol diglycidyl ether with an epoxy equivalent of 100 to 600 g / eq, polypropylene glycol diglycidyl ether with an epoxy equivalent of 200 to 800 g / eq, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, dipropylene glycol diglycidyl ether and dimer acid diglycidyl ester.

6. A phenolic amine adduct according to any one of claims 1 to 3, It is characterized in that The end-capping agent is selected from one or more of butyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether, C12-14 alkyl glycidyl ether, neodecanoic acid glycidyl ester, and cardanol glycidyl ether.

7. A method for preparing a phenolic amine adduct as claimed in any one of claims 1 to 6, It is characterized in that The following steps are involved: Step 1) After aminophenol and a chain extender are mixed, the mixture is heated to a certain temperature to react to obtain an intermediate, and then a capping agent is added and mixed to obtain a dropwise solution; Step 2) adding the dropwise addition liquid to the heated raw material amine within a set time to react and keep the temperature, and obtaining a phenolic amine adduct after the temperature is kept.

8. The method for preparing a phenolic amine adduct according to claim 7, It is characterized in that The specific process of the reaction in step 1) is: heating to 80-120°C and keeping warm for 4-8 hours; The specific process of the reaction in step 2) is: the temperature of the bottom liquid of the kettle is raised to 60-90°C, the temperature of the dropwise liquid is maintained at 20-40°C, the dropwise addition is performed for 1-4 hours, and after the dropwise addition is completed, the temperature is maintained at 60-90°C for 1-4 hours to obtain a phenolic amine adduct.

Citation Information

Patent Citations

  • Preparation method of novel Mannich water-based epoxy curing agent

    CN102516502A