Preparation method of carbamate saturated polyester, carbamate saturated polyester and baking varnish

The preparation of carbamate saturated polyester by reaction of cyclic carbonate and organic alcohol amine solves the high cost and environmental protection problems caused by isocyanate in traditional methods, and achieves low-cost, environmentally friendly preparation of carbamate saturated polyester, and in Provides good adhesion and cohesion strength in baking paint.

CN118909234APending Publication Date: 2024-11-08SHENZHEN FEIYANG JUNYAN TECH DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093152.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The use of isocyanate in traditional methods of preparation of urethanes leads to high costs and environmental protection problems. Especially when the environmental protection pressure increases, the use of isocyanate raw materials will be subject to transportation, warehousing and environmental approvals.

Method used

Carbamate polyols are prepared by reaction of cyclic carbonate and organic alcohol amine, and then carbamate saturated polyester is prepared by catalytic esterification reaction, avoiding the use of isocyanate, and a more environmentally friendly and low-cost chemical preparation method is adopted.

Benefits of technology

The preparation of urethane saturated polyester is achieved without isocyanate, with low cost, mild process, no waste gas or waste liquid production, and the cyclic carbonate used is a green chemical, which improves the environmental protection of production and is in the paint. Provides good adhesion and cohesion strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a synthetic method of carbamic acid ester saturated polyester and a preparation method for using the carbamic acid ester saturated polyester as baking varnish, and belongs to the technical field of preparation of saturated polyester. Comprising the following preparation steps: S1, synthesizing carbamate polyol: adding cyclic carbonate into organic alcohol amine according to a molar ratio of (1.0-1.05): 1, and naturally reacting under the protection of nitrogen to obtain the carbamate polyol; the organic alcohol amine is alcohol amine containing one primary amine or secondary amine; s2, synthesis of carbamate saturated polyester: carrying out esterification reaction on carbamate polyol and dibasic acid or anhydride or dibasic acid ester in a molar ratio of (1.0-1.05): 1 under the condition of a catalyst to obtain the carbamate saturated polyester, so as to achieve the purpose of synthesizing the carbamate saturated polyester by adopting relatively more environment-friendly raw materials without using isocyanate; and the cost is also relatively low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of saturated polyesters, in particular to a preparation method of carbamate saturated polyester and carbamate saturated polyester baking varnish. Background Art

[0002] The polyester resin used in coatings is generally a low molecular weight, amorphous, branched, cross-linked polymer. Polyester resin is generally made from polyols and polyacids, and has two structures: pure linear and branched. The paint film prepared with pure linear resin has good flexibility and processing performance, while the paint film prepared with branched resin has outstanding hardness and weather resistance. When synthesizing polyester resin, if some other structures are introduced through chemical modification, the polyester resin can have properties that it does not originally have, so as to achieve the purpose of improving and highlighting certain properties, thereby achieving special application performance requirements.

[0003] Urethane is an important polymer material with excellent properties such as high strength, good wear resistance, good chemical resistance, high elasticity, and weather resistance, so it is widely used. The traditional preparation of urethane requires the use of isocyanates, and a small amount of blocked isocyanates are often added to baking varnish to improve performance. The use of blocked isocyanates leads to high costs on the one hand, and isocyanates are highly toxic and hazardous chemicals on the other hand. There are safety and environmental risks in production, storage, and transportation. Especially in the context of increasing environmental pressure, the use of isocyanate raw materials will be restricted by transportation, storage, and environmental approval. Therefore, it is necessary to invent a more environmentally friendly preparation method to avoid the use of isocyanates. Summary of the invention

[0004] In order to overcome the defects of high cost and environmental problems caused by the use of isocyanate in the above-mentioned preparation methods of the prior art, the present invention provides a preparation method of carbamate saturated polyester, which does not require the use of isocyanate and uses relatively more environmentally friendly raw materials to synthesize carbamate saturated polyester, and the cost is also low.

[0005] The first object of the present invention is to provide a method for preparing a saturated carbamate polyester, which adopts the following technical scheme: A method for preparing a saturated carbamate polyester, comprising the following preparation steps: S1. Synthesis of carbamate polyol: adding a cyclic carbonate in a molar ratio of (1.0-1.05):1 to an organic alcohol amine, and reacting naturally under nitrogen protection to obtain a carbamate polyol; the organic alcohol amine is an alcohol amine containing a primary amine or a secondary amine; S2. Synthesis of saturated carbamate polyester: esterify carbamate polyol with a molar ratio of (1.0-1.05):1 with dibasic acid or acid anhydride or dibasic acid ester in the presence of a catalyst to obtain saturated carbamate polyester.

[0006] Preferably, the cyclic carbonate is one or more of ethylene carbonate, propylene carbonate and glycerol carbonate.

[0007] Preferably, the organic alcohol amine is one or both of monoethanolamine and diethanolamine.

[0008] Preferably, the reaction temperature of the cyclic carbonate and the organic alcohol amine in step S1 is 30-60°C.

[0009] Preferably, the dibasic acid or anhydride or dibasic ester in step S2 is one or more of adipic acid, maleic anhydride, phthalic anhydride, acetic anhydride, dimethyl oxalate, dimethyl succinate, dimethyl adipate, and dimethyl phthalate.

[0010] Preferably, the temperature of the esterification reaction in step S2 is 80-120° C., and the reaction time is 3-6 hours.

[0011] Preferably, the catalyst in step S2 is one or more of sulfuric acid, phosphoric acid, p-toluenesulfonic acid, and solid acid.

[0012] The second object of the present invention is to provide a saturated carbamate polyester obtained by the preparation method of the saturated carbamate polyester described above.

[0013] The third object of the present invention is to provide a baking varnish, which comprises 1-2% of an additive, 10-20% of a solvent, and the remainder is the saturated polyester carbamate and the amino resin in claim 8, and the baking varnish is obtained after curing at 120-150°C for 10-15 minutes, wherein the weight ratio of the saturated polyester carbamate and the amino resin is (2-3):1.

[0014] In summary, the present invention has the following beneficial effects: in the preparation method of the carbamate saturated polyester provided by the present invention, there is no need to use isocyanate, relatively more environmentally friendly raw materials and chemical preparation methods are adopted, carbamate polyols are prepared by reacting cyclic carbonates and organic alcohol amines, and then carbamate saturated polyesters are prepared by catalytic esterification, the cost is relatively low, and the ring-opening reaction conditions of cyclic carbonates and organic alcohol amines are mild, without the generation of any waste gas and waste liquid, which is conducive to industrial production, so it is more environmentally friendly. And the cyclic carbonate used in this application, such as ethylene carbonate, propylene carbonate, glycerol carbonate, etc., belong to green chemicals, which can be prepared by reacting ethylene oxide or propylene oxide with carbon dioxide, and ethylene carbonate, propylene carbonate, etc. are less restricted in environmental protection relative to isocyanate, not only safer, but also because the reaction raw materials use carbon dioxide, it is also a very green chemical reaction.

[0015] The saturated carbamate polyester obtained in the present application is used as the main component of the baking varnish, and then combined with an amino resin. After curing at 120-150° C., the paint film has good adhesion and excellent cohesive strength. DETAILED DESCRIPTION

[0016] The present invention is further described in detail below with reference to the embodiments.

[0017] The raw materials used in this application are all commercially available.

[0018] A method for preparing a saturated carbamate polyester comprises the following steps: S1. Synthesis of carbamate polyol: adding cyclic carbonate in a molar ratio of 1:1 to an organic alcohol amine, and reacting naturally under nitrogen protection to obtain a carbamate polyol; the organic alcohol amine is an alcohol amine containing a primary amine or a secondary amine; S2. Synthesis of saturated carbamate polyester: Carbamate polyol with a molar ratio of 1:1 is subjected to an esterification reaction with a dibasic acid or anhydride or a dibasic acid ester in the presence of a catalyst to obtain a saturated carbamate polyester.

[0019] Preferably, the cyclic carbonate is one or more of ethylene carbonate, propylene carbonate and glycerol carbonate.

[0020] Preferably, the organic alcohol amine is one or both of monoethanolamine and diethanolamine.

[0021] Preferably, the reaction temperature of the cyclic carbonate and the organic alcohol amine in step S1 is 30-60°C.

[0022] Preferably, the dibasic acid or anhydride or dibasic ester in step S2 is one or more of dimethyl oxalate, dimethyl succinate, dimethyl adipate, dimethyl phthalate, adipic acid, maleic anhydride, phthalic anhydride, and acetic anhydride. Since the effects achieved are basically the same, only dimethyl oxalate and phthalic anhydride are listed in the embodiments of the present application.

[0023] Preferably, the temperature of the esterification reaction in step S2 is 80-120° C., and the reaction time is 3-6 hours.

[0024] Preferably, the catalyst in step S2 is one or more of sulfuric acid, phosphoric acid, p-toluenesulfonic acid, and solid acid. Since the catalytic effects achieved are basically the same, only p-toluenesulfonic acid is listed in the examples of the present application.

[0025] Example 1 A method for preparing a saturated carbamate polyester comprises the following steps: S1. Synthesis of carbamate polyol: 61 g (1 mol) of monoethanolamine was added to a four-necked flask, nitrogen was passed through, and the mixture was heated to 30 ° C with stirring. 88 g (1 mol) of ethylene carbonate was slowly added dropwise with continuous stirring for half an hour, and the mixture was naturally reacted at 30 ° C for 4 hours to obtain a carbamate polyol; S2. Synthesis of saturated carbamate polyester: 149 g (1 mol) of the carbamate polyol obtained in step S1 and 0.5 g of p-toluenesulfonic acid are added to a four-necked flask, a reflux condenser is installed, 118 g (1 mol) of dimethyl oxalate is added, the mixture is heated to 80°C, and the reaction is stirred continuously for 6 hours until 98.3% of the theoretical value of methanol is evaporated, and the reaction is stopped to obtain saturated carbamate polyester.

[0026] Example 2 A method for preparing a saturated carbamate polyester comprises the following steps: S1. Synthesis of carbamate polyol: 61 g (1 mol) of monoethanolamine was added to a four-necked flask, nitrogen was passed through, and the mixture was heated to 40 ° C with stirring. 123.9 g (1.05 mol) of glycerol carbonate was slowly added dropwise with continuous stirring for half an hour, and the mixture was naturally reacted at 40 ° C for 4 hours to obtain a carbamate polyol; S2. Synthesis of saturated carbamate polyester: 184.9 g (1 mol) of the carbamate polyol obtained in step S1 and 1.0 g of p-toluenesulfonic acid are added to a four-necked flask, a reflux condenser is installed, 118 g (1 mol) of dimethyl oxalate is added, the mixture is heated to 115°C, and the reaction is stirred continuously for 4 hours until 98.3% of the theoretical value of methanol is evaporated, and the reaction is stopped to obtain saturated carbamate polyester.

[0027] Example 3 A method for preparing a saturated carbamate polyester comprises the following steps: S1. Synthesis of carbamate polyol: 105 g (1 mol) of diethanolamine was added to a four-necked flask, nitrogen was passed through, and the mixture was heated to 50 ° C with stirring. 88 g (1 mol) of ethylene carbonate was slowly added dropwise with continuous stirring for half an hour, and the mixture was naturally reacted at 50 ° C for 4 hours to obtain a carbamate polyol; S2. Synthesis of saturated carbamate polyester: 202.65 g (1.05 mol) of the carbamate polyol obtained in step S1 and 1.5 g of p-toluenesulfonic acid are added to a four-necked flask, a reflux condenser is installed, 118 g (1 mol) of dimethyl oxalate is added, the mixture is heated to 120°C, and the reaction is stirred continuously for 3 h until 98.3% of the theoretical value of methanol is evaporated, and the reaction is stopped to obtain saturated carbamate polyester.

[0028] Example 4 A method for preparing a saturated carbamate polyester comprises the following steps: S1. Synthesis of carbamate polyol: 105 g (1 mol) of diethanolamine was added to a four-necked flask, nitrogen was passed through, and the mixture was heated to 60 ° C with stirring. 118 g (1 mol) of glycerol carbonate was slowly added dropwise with continuous stirring for half an hour, and the mixture was naturally reacted at 60 ° C for 4 hours to obtain a carbamate polyol; S2. Synthesis of saturated carbamate polyester: Add 223 g (1 mol) of the carbamate polyol obtained in step S1 and 2.5 g of p-toluenesulfonic acid into a four-necked flask, install a reflux condenser, add 118 g (1 mol) of dimethyl oxalate, heat to 120°C, stir and react for 3 hours until 98.3% of the theoretical value of methanol is evaporated, then stop the reaction to obtain saturated carbamate polyester.

[0029] Example 5 A method for preparing a saturated carbamate polyester comprises the following steps: S1. Synthesis of carbamate polyol: 61 g (1 mol) of monoethanolamine was added to a four-necked flask, nitrogen was passed through, and the mixture was heated to 40 ° C with stirring. 88 g (1 mol) of ethylene carbonate was slowly added dropwise with continuous stirring for half an hour, and the mixture was naturally reacted at 40 ° C for 4 hours to obtain a carbamate polyol; S2. Synthesis of saturated carbamate polyester: 149 g (1 mol) of the carbamate polyol obtained in step S1 and 0.5 g of p-toluenesulfonic acid are added to a four-necked flask, a reflux condenser is installed, 148 g (1 mol) of phthalic anhydride is added, the mixture is heated to 80°C, and the reaction is stirred continuously for 6 hours until 98.3% of the theoretical value of methanol is evaporated, and the reaction is stopped to obtain saturated carbamate polyester.

[0030] Example 6 A method for preparing a saturated carbamate polyester comprises the following steps: S1. Synthesis of carbamate polyol: 61 g (1 mol) of monoethanolamine was added to a four-necked flask, nitrogen was passed through, and the mixture was heated to 40 ° C with stirring. 102 g (1 mol) of propylene carbonate was slowly added dropwise with continuous stirring for half an hour, and the mixture was naturally reacted at 40 ° C for 4 hours to obtain a carbamate polyol; S2. Synthesis of saturated carbamate polyester: 163 g (1 mol) of the carbamate polyol obtained in step S1 and 0.5 g of p-toluenesulfonic acid are added to a four-necked flask, a reflux condenser is installed, 146 g (1 mol) of adipic acid is added, the mixture is heated to 80°C, and the reaction is stirred continuously for 6 hours until 98.3% of the theoretical value of methanol is evaporated, and the reaction is stopped to obtain saturated carbamate polyester.

[0031] Application Example 1 A baking varnish comprises 60% of the saturated urethane polyester obtained in Example 1, 20% of hexamethoxymethyl melamine resin, 1% of BYK-333 leveling agent, 15% of propylene glycol methyl ether and 4% of ethanol. After stirring and mixing, the baking varnish is cured at 120° C. for 15 minutes.

[0032] Application Example 2 A baking varnish comprises 60% of the saturated urethane polyester obtained in Example 2, 20% of hexamethoxymethyl melamine resin, 1% of BYK-333 leveling agent, 15% of propylene glycol methyl ether and 4% of ethanol. After stirring and mixing, the mixture is cured at 150° C. for 10 minutes to obtain the baking varnish.

[0033] Application Example 3 A baking varnish comprises 60% of the saturated urethane polyester obtained in Example 3, 20% of hexamethoxymethyl melamine resin, 1% of BYK-333 leveling agent, 15% of propylene glycol methyl ether and 4% of ethanol. After stirring and mixing, the baking varnish is cured at 120° C. for 15 minutes.

[0034] Application Example 4 A baking varnish comprises 60% of the saturated urethane polyester obtained in Example 4, 20% of hexamethoxymethyl melamine resin, 1% of BYK-333 leveling agent, 15% of propylene glycol methyl ether and 4% of ethanol. After stirring and mixing, the mixture is cured at 120° C. for 15 minutes to obtain the baking varnish.

[0035] Application Example 5 A baking varnish comprises 60% of the saturated urethane polyester obtained in Example 5, 20% of hexamethoxymethyl melamine resin, 1% of BYK-333 leveling agent, 15% of propylene glycol methyl ether and 4% of ethanol. After stirring and mixing, the baking varnish is cured at 120° C. for 15 minutes.

[0036] Application Example 6 A baking varnish comprises 60% of the saturated polyester of carbamate obtained in Example 6, 20% of hexamethoxymethyl melamine resin, 1% of BYK-333 leveling agent, 15% of propylene glycol methyl ether and 4% of ethanol. After stirring and mixing, the mixture is cured at 120° C. for 15 minutes to obtain the baking varnish.

[0037] Application Example 7 A baking varnish comprises 58% of the saturated polyester of carbamate obtained in Example 6, 29% of hexamethoxymethyl melamine resin, 2% of BYK-333 leveling agent, 10% of propylene glycol methyl ether and 1% of ethanol. After stirring and mixing, the mixture is cured at 120° C. for 15 minutes to obtain the baking varnish.

[0038] Comparative application example 1 A baking varnish, which is different from Application Example 1 in that Changxing ETERKYD5050-B-75 saturated polyester (solid content of 75%, viscosity of 910 mPa·s, 25°C) is used to replace the urethane saturated polyester in Application Example 1, and the rest is the same as Application Example 1.

[0039] Application Comparative Example 2 A baking varnish, which is different from Application Example 1 in that it includes 20% of the urethane saturated polyester obtained in Example 1, 40% of Changxing ETERKYD5050-B-75 saturated polyester, 20% of hexamethoxymethyl melamine resin, 1% of BYK-333 leveling agent, 15% of propylene glycol methyl ether, and 4% of ethanol. After stirring and mixing, the baking varnish is obtained after curing at 120° C. for 15 minutes.

[0040] Application Comparative Example 3 A baking varnish, which is different from Application Example 1 in that it includes 30% of the urethane saturated polyester obtained in Example 1, 30% of Changxing ETERKYD5050-B-75 saturated polyester, 20% of hexamethoxymethyl melamine resin, 1% of BYK-333 leveling agent, 15% of propylene glycol methyl ether, and 4% of ethanol. After stirring and mixing, the baking varnish is obtained after curing at 120° C. for 15 minutes.

[0041] Performance Testing The baking varnish obtained from the above application examples and the application comparison examples was tested for solid content, viscosity, hardness, glossiness, adhesion, and flexibility. The test results are shown in Table 1.

[0042] The solid content test is carried out in accordance with the relevant provisions of GB / T9272-1988; the viscosity test is carried out in accordance with the relevant provisions of GB / T1723-1993 "Determination of Coating Viscosity"; the hardness test is carried out in accordance with the relevant provisions of GB / T6739-1996 "Determination of Smear Hardness Pencil"; the gloss test is carried out in accordance with the relevant provisions of GB1743-1979 "Determination of Paint Film Gloss"; the flexibility test is carried out in accordance with GB / T6742-2007 "Bending Test for Paints and Varnishes (Cylindrical Shaft)", and the adhesion is tested by the cross-hatch method, with 0 being the best and 5 being the worst.

[0043] The water resistance was tested with reference to the relevant provisions of GB / T1733-1993 "Determination of water resistance of paint films". The appearance and adhesion were observed after boiling in water for 1 hour. The test results are shown in Table 2.

[0044] Table 1 Paint performance test results Table 2 Test results of paint water resistance It can be seen from Table 1 and Table 2 that after the saturated carbamate polyester prepared in the examples of the present application is applied to the baking varnish, the baking varnish obtained in Application Examples 1-7 has good adhesion and flexibility on steel, stainless steel and aluminum plates, and after 1 hour of boiling in water, the baking varnish films of Application Examples 1-7 of the present application still have good adhesion and no change in appearance. This shows that the saturated carbamate polyester prepared by the method of the present application still has good performance in baking varnish without using isocyanate.

[0045] Compared with Application Example 1, when an equal amount of commercially available saturated polyester is used to replace the saturated carbamate polyester in the present application, the adhesion, flexibility and viscosity of the baking varnish obtained in Application Example 1 are reduced, and after 1 hour of boiling in water, the adhesion of the paint film of Application Example 1 is reduced, and the surface of the paint film also changes, which can further illustrate that the saturated carbamate polyester obtained in the present application has excellent adhesion, flexibility and water resistance after being applied to the baking varnish.

[0046] Compared with Application Example 1, when the total amount of polyester remains unchanged and the weight ratio of commercially available saturated polyester to carbamate saturated polyester is 2:1, the adhesion of the paint film of Application Example 2 to stainless steel and aluminum plates is reduced, and the flexibility is also reduced. After a 1-hour water boiling test, the adhesion and hardness of the paint film of Application Example 2 to steel are reduced; when the total amount of polyester remains unchanged and the weight ratio of commercially available saturated polyester to carbamate saturated polyester is 1:1, the adhesion of the paint film of Application Example 3 to stainless steel and aluminum plates is reduced, and the flexibility is also reduced. After the water boiling test, the adhesion of the paint film of Application Example 3 to steel is reduced. It can be seen that when the polyester in the baking paint is completely made of the carbamate saturated polyester obtained in the embodiment of the present application, the adhesion, flexibility and other properties of the paint film can be effectively improved.

[0047] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for synthesizing a saturated carbamate polyester, characterized in that: The method comprises the following preparation steps: S1. Synthesis of carbamate polyol: adding cyclic carbonate in a molar ratio of (1.0-1.05):1 to organic alcohol amine, and reacting naturally under nitrogen protection to obtain carbamate polyol; the organic alcohol amine is an alcohol amine containing a primary amine or a secondary amine; S2. Synthesis of saturated carbamate polyester: Carbamate polyol with a molar ratio of (1.0-1.05):1 is subjected to esterification reaction with a dibasic acid or anhydride or a dibasic acid ester in the presence of a catalyst to obtain a saturated carbamate polyester.

2. The method for synthesizing a saturated carbamate polyester according to claim 1, characterized in that: The cyclic carbonate is one or more of ethylene carbonate, propylene carbonate and glycerol carbonate.

3. The method for synthesizing a saturated carbamate polyester according to claim 1, characterized in that: The organic alcohol amine is one or both of monoethanolamine and diethanolamine.

4. The method for synthesizing a saturated carbamate polyester according to claim 1, characterized in that: The reaction temperature of the cyclic carbonate and the organic alcohol amine in step S1 is 30-60°C.

5. The method for synthesizing a saturated carbamate polyester according to claim 1, characterized in that: In step S2, the dibasic acid or anhydride or dibasic ester is one or more of adipic acid, maleic anhydride, phthalic anhydride, acetic anhydride, dimethyl oxalate, dimethyl succinate, dimethyl adipate, and dimethyl phthalate.

6. The method for synthesizing a saturated carbamate polyester according to claim 1, characterized in that: The temperature of the esterification reaction in step S2 is 80-120° C., and the reaction time is 3-6 hours.

7. The method for synthesizing a saturated carbamate polyester according to claim 1, characterized in that: The catalyst in step S2 is one or more of sulfuric acid, phosphoric acid, p-toluenesulfonic acid, and solid acid.

8. A saturated carbamate polyester obtained by the method for synthesizing a saturated carbamate polyester as claimed in any one of claims 1 to 7.

9. A baking varnish, characterized in that: The composition comprises 1-2% of an auxiliary agent, 10-20% of a solvent, and the balance of the saturated polyester carbamate and the amino resin in claim 8. The baking varnish is obtained after curing at 120-150° C. for 10-15 minutes. The weight ratio of the saturated polyester carbamate and the amino resin is (2-3):1.