Preparation method of low-smoke and high-modulus PC / ABS alloy halogen-free flame-retardant material and phosphorus-silicon-containing flame retardant
By using phosphorus-containing silicon flame retardant in PC/ABS alloys, the ceramic barrier layer is formed, which solves the problem of smoke and harmful gas generation during combustion of traditional flame retardant materials, and achieves low smoke and high modulus halogen-free resistance Fueling effect, suitable for a variety of industrial applications.
Patent Information
- Application Number
- CN202411334443.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-24
AI Technical Summary
Existing PC/ABS alloy flame retardant materials produce a large amount of thick smoke and harmful gases when burned, and traditional halogen flame retardants pose a threat to the environment and human health, making it difficult to meet the requirements of modern industry for high modulus, low smoke and environmental protection.
Using phosphorus-containing silicon flame retardant, a new flame retardant containing both phosphorus and silicon elements was synthesized and added to PC/ABS alloys, low smoke and high modulus were prepared through acid catalysts and specific process conditions. Halogen-free flame retardant material uses the synergistic effect of phosphorus and silicon to form a ceramic barrier layer to inhibit flame propagation and smoke generation.
It has achieved significant reduction in the generation of smoke and harmful gases without reducing the material modulus, improved flame retardant performance and safety, and is suitable for automotive instrument displays, household appliances and rail transit interior parts and other fields.
Smart Images

Figure BDA0005057881830000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy flame retardant materials, and in particular to a preparation method of a low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material and a phosphorus-silicon flame retardant. Background Art
[0002] In modern industry, polycarbonate / acrylonitrile-butadiene-styrene (PC / ABS) alloy has become an ideal material in the fields of electronics, automobile industry, and home appliance casings due to its excellent comprehensive properties, such as good mechanical strength, heat resistance, dimensional stability, and impact toughness. However, with the increasing complexity of application scenarios, especially in the field of electronics, higher flame retardancy, safety, and environmental protection requirements are placed on materials. Traditional PC / ABS alloy flame retardant materials mostly use halogen flame retardants, such as bromides and chlorides. These materials may release toxic and harmful hydrogen halide gases and carcinogens such as dioxins during combustion, which seriously threaten human health and cause irreversible damage to the environment. Therefore, the development of a halogen-free, low-smoke, high-modulus flame retardant material has become an important research direction in current materials science.
[0003] Halogen-free flame retardant materials are gaining more and more attention due to their environmental advantages. Traditional halogen flame retardants produce a lot of smoke and harmful gases when burning, while halogen-free flame retardants can achieve high-efficiency flame retardant effects while significantly reducing the generation of smoke and harmful substances. They are particularly suitable for fields with strict environmental requirements. The core of halogen-free flame retardant technology is to use environmentally friendly flame retardants that replace halogens, such as phosphorus-based, nitrogen-based, and silicon-based flame retardants. They do not produce toxic gases during combustion and provide protection through a variety of flame retardant mechanisms, such as the formation of a condensed phase carbonization layer and the capture of active free radicals in the gas phase, thereby inhibiting the spread and development of flames.
[0004] Among the many halogen-free flame retardant systems, the phosphorus-silicon synergistic flame retardant system exhibits unique advantages. Phosphorus-based flame retardants can promote the formation of a dense carbonized layer on the surface of the material under high temperature conditions, effectively isolating heat and oxygen and preventing further combustion. Silicon-based flame retardants generate a protective layer of silicon dioxide (SiO) at high temperatures to enhance the heat resistance and fire resistance of the material. The synergistic effect of phosphorus-silicon flame retardants can not only effectively improve the flame retardant properties of PC / ABS alloys, but also reduce the generation of smoke and improve safety during the combustion process. In addition, the phosphorus-silicon flame retardant system has little effect on the mechanical properties of PC / ABS materials, can maintain or improve the high modulus characteristics of the material, and adapt to application scenarios with high requirements for strength and rigidity.
[0005] In the development process of halogen-free flame-retardant PC / ABS alloy materials, in addition to flame retardancy and environmental protection, the mechanical properties of the materials, especially the modulus, need to be taken into account. High modulus PC / ABS alloy materials have better rigidity and load-bearing capacity in applications, and are particularly suitable for automotive interior and exterior trims, electronic and electrical equipment housings, and other occasions that have high requirements for strength, rigidity, and durability. Therefore, the research of low-smoke, high-modulus halogen-free flame-retardant PC / ABS alloy materials has important technical and market value.
[0006] Current research focuses on improving the flame retardancy and mechanical properties of PC / ABS alloys by introducing different types of phosphorus and silicon flame retardants. Phosphorus flame retardants can form a stable glassy or ceramic carbonized layer through dehydration condensation during the combustion process, effectively isolating heat sources and oxygen and preventing flame propagation; the silicon dioxide layer generated by silicon flame retardants during combustion can further improve the thermal stability of the material and reduce the spread of flames. By rationally designing the phosphorus-silicon ratio, flame retardants can achieve excellent flame retardant effects at lower addition levels while maintaining the high modulus and low smoke characteristics of the material.
[0007] In the specific preparation process, the uniform dispersion of phosphorus silicon flame retardants and their compatibility with PC / ABS matrix materials are key technical challenges. The uniformity and compatibility of flame retardants directly affect the final performance of flame retardant materials. In order to ensure the effective dispersion of flame retardants in PC / ABS alloys, it is usually necessary to enhance the interface bonding between flame retardants and matrix resins through surface modification technology or the use of specific dispersants. In addition, process parameters such as processing temperature, pressure, mixing speed, etc. also need to be precisely optimized to ensure the thermal stability, mechanical properties and flame retardant properties of the material during processing.
[0008] In addition, low smoke characteristics are also one of the key performance indicators in the development of modern flame retardant materials. The smoke produced by flame retardant materials during combustion not only affects the visibility at the fire scene, but also poses serious health risks. By adjusting the chemical structure of phosphorus silicon flame retardants and their dispersion state in the material, the smoke density during combustion can be significantly reduced, thereby improving the safety of the material.
[0009] Chinese patent CN102604315A discloses a low smoke density PC / ABS alloy for automotive interior parts and a preparation method thereof. The low smoke density PC / ABS alloy is compounded with four flame retardants and smoke suppressants such as zinc borate, molybdenum trioxide, ammonium octamolybdate and zinc molybdate. In the PC / ABS alloy, not only the flame retardant effect is effectively improved, but also the smoke density is more effectively reduced and smoke is efficiently suppressed. However, molybdenum compounds such as molybdenum trioxide, ammonium octamolybdate and zinc molybdate are also used in this patent. Chinese patent CN112111142A discloses a low smoke density, flame retardant PC / ABS alloy material and a preparation method thereof, which uses polydimethylsiloxane, zinc borate, and 10-12 parts of phosphate flame retardant flame retardant, which reduces the smoke density while sacrificing a part of the mechanical strength of the alloy. Chinese patent CN106995602A discloses a high modulus, high flow, halogen-free, flame-retardant PC / ABS alloy material and a preparation method thereof, which uses carbon fiber as a reinforcing material, polyaromatic ester phosphates and ultrafine phosphates as flame retardants, silicon-based triazine as a carbon-forming synergist, and MBS toughening agent, wherein the PX200 flame retardant exceeds 10 parts, which affects the modulus of the alloy itself to a certain extent. Summary of the invention
[0010] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a phosphorus-silicon flame retardant, by which a new flame retardant containing both phosphorus and silicon elements can be synthesized, and the new flame retardant is added to PC / ABS alloy to prepare a low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material.
[0011] Another object of the present invention is to provide a low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material, which improves the flame retardancy of PC / ABS material by adding phosphorus-containing silicon flame retardant, reduces the amount of traditional phosphate flame retardant, and reduces the influence on the tensile strength, bending modulus and thermal deformation temperature of the alloy; in addition, the phosphorus-containing silicon flame retardant itself is highly compatible with PC / ABS, and is easy to react with zinc borate, triphenyl boric acid and octamolybdenum during combustion to form a ceramic barrier layer, which has the functions of smoke suppression, flame retardancy and preventing molten body from dripping, and the prepared flame retardant material can be widely used in the production of automobile instrument display housings, household appliances, communication electronic and electrical components and rail transit interior decoration parts.
[0012] The purpose of the present invention is achieved by the following technical solution: A method for preparing a phosphorus-silicon flame retardant comprises the following steps:
[0013] S1. Add phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double end cap into a mixed system of methanol and water in proportion, stir evenly, add an acidic catalyst, adjust the pH value to 4-6, control the temperature at 0°C to 45°C to react for 8-12h, neutralize, wash, and degas at -0.098MPa, 85°C to obtain an intermediate for standby use;
[0014] S2. Add DOPO flame retardant in an equal molar ratio to the vinyl in the vinyl double head and DMF in an equal mass ratio to the intermediate to the intermediate obtained in step S1, heat to 60°C to 75°C for 4 to 12 hours, filter, wash and dry to obtain a phosphorus-containing silicon flame retardant.
[0015] The phosphorus-silicon flame retardant in the present invention is prepared by the above method, and a new flame retardant containing both phosphorus and silicon elements can be synthesized by the above method, and the new flame retardant is added to PC / ABS alloy to prepare a low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material.
[0016] In addition, the present invention can also carry out balanced polycondensation of two of phenyltrimethoxysiloxane, diphenyldimethoxysilane, methylphenyldimethoxysilane, and dimethyldimethoxy with ethylene dicapped or tetramethyltetravinylcyclotetrasiloxane in an alcohol aqueous solution according to the above proportion under acidic conditions, and then react with 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and a solvent under heating conditions for several hours, and add a non-polar solvent to obtain a phosphorus-containing silicon flame retardant.
[0017] Preferably, the phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double head are mixed in a molar ratio of 0.1-3:0.5-4:0.1-0.5; and the methanol and water are mixed in a mass ratio of 1:0.8-1.2 to form a mixed system.
[0018] Preferably, the mass ratio of the mixture of phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double-capped silane to the mixed system of methanol and water is 1:0.8-1.2.
[0019] Preferably, the phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double head are mixed in a molar ratio of 0.1-1:0.5-4:0.1-0.4, and the solid content thereof is 35%-60%.
[0020] Preferably, the acidic catalyst is at least one of benzenesulfonic acid, p-toluenesulfonic acid, sulfuric acid, hydrochloric acid, trifluoromethanesulfonic acid, methanesulfonic acid, dodecylbenzenesulfonic acid, phosphoric acid, and strong acid hydrogen salts.
[0021] The present invention also provides a low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material, comprising the following raw materials in parts by weight: 30 to 60 parts of PC resin, 5 to 30 parts of ABS resin, 1 to 3 parts of silicone synergistic flame retardant additives, 1 to 3 parts of silicone toughening agents, 3 to 5 parts of phosphorus-containing silicon flame retardants, 0.1 to 2 parts of sulfonate flame retardants, 1 to 5 parts of zinc borate, 1 to 3 parts of triphenyl boric acid, 0.1 to 0.5 parts of octamolybdenum, 0.5 to 3 parts of phosphate flame retardants, 0.1 to 0.5 parts of anti-dripping agents, 0.3 to 1 parts of antioxidants, 0.2 to 0.5 parts of ultraviolet absorbers, and 0.5 to 1 parts of lubricants.
[0022] The present invention improves the flame retardancy of PC / ABS materials by adding phosphorus-containing silicon flame retardants to combustible materials, reduces the amount of traditional phosphate flame retardants used, and reduces the influence on the tensile strength, bending modulus and thermal deformation temperature of the alloy; in addition, the phosphorus-containing silicon flame retardant itself is highly compatible with PC / ABS, and is easy to react with zinc borate, triphenyl boric acid and octamolybdenum during combustion to form a ceramic barrier layer, which has the functions of smoke suppression, flame retardancy and preventing molten body from dripping, and the prepared flame retardant material can be widely used in the production of automobile instrument display housings, household appliances, communication electronic and electrical parts and rail transportation interior decoration parts.
[0023] Preferably, the melt index of the PC resin is 8 to 12 g / 10 min.
[0024] Preferably, the organosilicon synergistic flame retardant additive is phenyl silsesquioxane, preferably SIFR-907 or SIFR-908 provided by QuanSheng Polycarbonate Technology Co., Ltd.
[0025] Preferably, the sulfonate flame retardant is selected from KKS-A2, 870M, 5100, 6100 of Quansheng or KSS, HES, HES-2 of Arichem.
[0026] Preferably, the organosilicon toughening agent is selected from at least one of USI3310, USI3305 and USI3306 of Quansheng.
[0027] Preferably, the anti-dripping agent is selected from at least one of KT-107, KT201 and KT-P205 of Quansheng.
[0028] Preferably, the phosphate flame retardant is at least one of FCR210, SPB-100, HM1100, PX200, and PX220.
[0029] Preferably, the antioxidant consists of a primary antioxidant and an auxiliary antioxidant, wherein the primary antioxidant is selected from at least one of antioxidant 1010, antioxidant 1076 and antioxidant MD-697; and the auxiliary antioxidant is selected from at least one of antioxidant 168 and antioxidant 412S.
[0030] The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method:
[0031] A1. Dry the PC resin at 120-130°C until the water content is less than 0.025% and set aside;
[0032] A2. Dry the ABS resin at 85-90°C until the water content is less than 0.025%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside.
[0033] A3. Add the mixed raw materials into a twin-screw extruder, and obtain flame-retardant PC / ABS material after extrusion and granulation; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 250-300 RPM.
[0034] The beneficial effect of the present invention is that: the present invention can synthesize a new flame retardant containing phosphorus and silicon elements at the same time through the method, and add the new flame retardant to PC / ABS alloy to prepare a low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material.
[0035] The invention discloses a low-smoke, high-modulus PC / ABS alloy halogen-free flame-retardant material. The flame retardancy of the PC / ABS material is improved by adding a phosphorus-silicon flame retardant, thereby reducing the amount of a traditional phosphate flame retardant and reducing the influence on the tensile strength, bending modulus and thermal deformation temperature of the alloy. In addition, the phosphorus-silicon flame retardant itself is highly compatible with PC / ABS and is easy to react with zinc borate, triphenyl boric acid and octamolybdenum during combustion to form a ceramic barrier layer, which has the functions of suppressing smoke, flame retardancy and preventing molten body from dripping. The prepared flame-retardant material can be widely used in the production of automobile instrument display housings, household appliances, communication electronic and electrical parts and rail transportation interior decoration parts. DETAILED DESCRIPTION
[0036] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0037] Example 1
[0038] A method for preparing a phosphorus-silicon flame retardant comprises the following steps:
[0039] S1. Add phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double end cap into a mixture of methanol and water in proportion, stir evenly, add an acidic catalyst, adjust the pH value to 4, control the temperature at 0°C to react for 12h, neutralize, wash, and degas at -0.098MPa, 85°C to obtain an intermediate for standby use;
[0040] S2. Add DOPO flame retardant in an equal molar ratio to the vinyl in the vinyl double head and DMF in an equal mass ratio to the intermediate to the intermediate obtained in step S1, heat to 60° C. to react for 12 hours, filter, wash and dry to obtain a phosphorus-containing silicon flame retardant.
[0041] The phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double head are mixed in a molar ratio of 0.1:0.5:0.1, and the solid content thereof is 35% to 60%.
[0042] The methanol and water form a mixed system in a mass ratio of 1:0.8.
[0043] The mass ratio of the mixture of phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double-capped silane to the mixed system of methanol and water is 1:0.8.
[0044] The acid catalyst is benzenesulfonic acid.
[0045] A low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material comprises the following raw materials in parts by weight: 30 parts of PC resin, 5 parts of ABS resin, 1 part of organic silicon synergistic flame retardant additive, 1 part of organic silicon toughening agent, 3 parts of phosphorus-containing silicon flame retardant, 0.1 part of sulfonate flame retardant, 1 part of zinc borate, 1 part of triphenyl boric acid, 0.1 part of octamolybdenum, 0.5 part of phosphate flame retardant, 0.1 part of anti-dripping agent, 0.3 part of antioxidant, 0.2 part of ultraviolet absorber and 0.5 part of lubricant.
[0046] The PC resin has a melt index of 8 g / 10 min.
[0047] The organosilicon synergistic flame retardant additive is phenyl silsesquioxane, preferably SIFR-907 provided by QuanSheng Polycarbonate Technology Co., Ltd.
[0048] The sulfonate flame retardant is selected from Quansheng KKS-A2.
[0049] The organosilicon toughening agent is selected from USI3310 produced by Quansheng.
[0050] The anti-dripping agent is selected from KT-107 of Quansheng.
[0051] The phosphate flame retardant is FCR210.
[0052] The antioxidant is composed of a primary antioxidant and an auxiliary antioxidant in a mass ratio of 1:1. The primary antioxidant is selected from antioxidant 1010; the auxiliary antioxidant is selected from antioxidant 168.
[0053] The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method:
[0054] A1. Dry the PC resin at 120°C until the water content is less than 0.025% and set aside;
[0055] A2. Dry the ABS resin at 85°C until the water content is less than 0.025%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside.
[0056] A3. Add the mixed raw materials into a twin-screw extruder, and extrude and granulate to obtain a flame-retardant PC / ABS material; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 300 RPM.
[0057] Example 2
[0058] A method for preparing a phosphorus-silicon flame retardant comprises the following steps:
[0059] S1. Add phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double end cap into a mixture of methanol and water in proportion, stir evenly, add an acidic catalyst, adjust the pH value to 5.5, control the temperature at 20°C to react for 10 hours, neutralize, wash, and degas at -0.098MPa, 85°C to obtain an intermediate for standby use;
[0060] S2. Add DOPO flame retardant in an equal molar ratio to the vinyl in the vinyl double head and DMF in an equal mass ratio to the intermediate to the intermediate obtained in step S1, heat to 65° C. to react for 8 hours, filter, wash and dry to obtain a phosphorus-containing silicon flame retardant.
[0061] The phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double head are mixed in a molar ratio of 2:2:3, and the solid content thereof is 35% to 60%.
[0062] The methanol and water form a mixed system in a mass ratio of 1:1.0.
[0063] The mass ratio of the mixture of phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double-capped silane to the mixed system of methanol and water is 1:1.0.
[0064] The acid catalyst is composed of sulfuric acid, hydrochloric acid and trifluoromethanesulfonic acid in a mass ratio of 1:1.0:1.0.
[0065] A low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material comprises the following raw materials in parts by weight: 45 parts of PC resin, 20 parts of ABS resin, 2 parts of organic silicon synergistic flame retardant additive, 2 parts of organic silicon toughening agent, 4 parts of phosphorus-containing silicon flame retardant, 1 part of sulfonate flame retardant, 3 parts of zinc borate, 2 parts of triphenyl boric acid, 0.3 parts of octamolybdenum, 1.5 parts of phosphate flame retardant, 0.3 parts of anti-dripping agent, 0.8 parts of antioxidant, 0.4 parts of ultraviolet absorber and 0.8 parts of lubricant.
[0066] The PC resin has a melt index of 10 g / 10 min.
[0067] The organosilicon synergistic flame retardant additive is phenyl silsesquioxane, preferably SIFR-908 provided by QuanSheng Polycarbonate Technology Co., Ltd.
[0068] The sulfonate flame retardant is selected from Quansheng 870M.
[0069] The organosilicon toughening agent is selected from USI3305 of Quansheng.
[0070] The anti-dripping agent is selected from KT201 of Quansheng.
[0071] The phosphate flame retardant is SPB-100.
[0072] The antioxidant is composed of a primary antioxidant and an auxiliary antioxidant in a mass ratio of 1:1.0. The primary antioxidant is selected from antioxidant 1076; the auxiliary antioxidant is selected from antioxidant 168.
[0073] The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method:
[0074] A1. Dry the PC resin at 125°C until the water content is less than 0.025% and set aside;
[0075] A2. Dry the ABS resin at 88°C until the water content is less than 0.025%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside.
[0076] A3. Add the mixed raw materials into a twin-screw extruder, and obtain a flame-retardant PC / ABS material after extrusion and granulation; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 280 RPM.
[0077] Example 3
[0078] A method for preparing a phosphorus-silicon flame retardant comprises the following steps:
[0079] S1. Add phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double end cap into a mixture of methanol and water in proportion, stir evenly, add an acidic catalyst, adjust the pH value to 6, control the temperature at 45°C to react for 12h, neutralize, wash, and degas at -0.098MPa, 85°C to obtain an intermediate for standby use;
[0080] S2. Add DOPO flame retardant in an equal molar ratio to the vinyl in the vinyl double head and DMF in an equal mass ratio to the intermediate to the intermediate obtained in step S1, heat to 75° C. and react for 12 hours, filter, wash and dry to obtain a phosphorus-containing silicon flame retardant.
[0081] The phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double head are mixed in a molar ratio of 3:4:0.5, and the solid content thereof is 35% to 60%.
[0082] The methanol and water form a mixed system in a mass ratio of 1:1.2.
[0083] The mass ratio of the mixture of phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double-capped silane to the mixed system of methanol and water is 1:1.2.
[0084] The acid catalyst is dodecylbenzenesulfonic acid.
[0085] A low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material comprises the following raw materials in parts by weight: 60 parts of PC resin, 30 parts of ABS resin, 3 parts of organic silicon synergistic flame retardant additive, 3 parts of organic silicon toughening agent, 5 parts of phosphorus-containing silicon flame retardant, 2 parts of sulfonate flame retardant, 5 parts of zinc borate, 3 parts of triphenyl boric acid, 0.5 parts of octamolybdenum, 3 parts of phosphate flame retardant, 0.5 parts of anti-dripping agent, 1 part of antioxidant, 0.5 parts of ultraviolet absorber and 1 part of lubricant.
[0086] The PC resin has a melt index of 12 g / 10 min.
[0087] The organosilicon synergistic flame retardant additive is phenyl silsesquioxane, preferably SIFR-907 provided by QuanSheng Polycarbonate Technology Co., Ltd.
[0088] The sulfonate flame retardant is selected from KSS of Arichem.
[0089] The organosilicon toughening agent is selected from USI3306 of Quansheng.
[0090] The anti-dripping agent is selected from KT-P205 of Quansheng.
[0091] The phosphate flame retardant is PX200.
[0092] The antioxidant is composed of a primary antioxidant and an auxiliary antioxidant in a ratio of 1:1. The primary antioxidant is selected from antioxidant MD-697; the auxiliary antioxidant is selected from antioxidant 412S.
[0093] The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method:
[0094] A1. Dry the PC resin at 130°C until the water content is less than 0.025% and set aside;
[0095] A2. Dry the ABS resin at 90°C until the water content is less than 0.025%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside.
[0096] A3. Add the mixed raw materials into a twin-screw extruder, and extrude and granulate to obtain a flame-retardant PC / ABS material; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 300 RPM.
[0097] Example 4
[0098] A method for preparing a phosphorus-silicon flame retardant comprises the following steps:
[0099] S1. Add 39.6g phenyltrimethoxysiloxane, 244.0g methylphenyldimethoxysilane and 55.8g vinyl double-end cap into a mixture of 339.4g methanol and water, stir evenly at room temperature for 30min, then add hydrochloric acid solution dropwise at about 20°C, adjust the pH value to 4.5, continue the reaction for 12h, then adjust to neutral with sodium carbonate, let stand and stratify, remove the waste liquid layer, wash 3 times to neutral, add 0.3% activated carbon, stir for 1h, filter, -0.098MPa, 120°C to obtain an intermediate for standby use; after taking the intermediate, calibrate the vinyl content by nuclear magnetic resonance method, 0.1mol / 100g;
[0100] S2. Take 100 g of the above-mentioned intermediate and add it to a mixed solution of DMF and toluene in a mass ratio of 3:7. Add equal amounts, stir evenly, then add 22.7 g DOPO, slowly heat to 70°C, react for 6 hours, cool, add an equal amount of methanol to precipitate to obtain a crude product, wash 3 times with deionized water, wash 3 times with isopropanol, and dry in an oven at 120°C with a yield of 98% to obtain a phosphorus-containing silicon flame retardant.
[0101] The methanol and water form a mixed system in a mass ratio of 1:1.2.
[0102] Example 5
[0103] A low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material comprises the following raw materials in parts by weight: 60 parts of PC resin, 30 parts of ABS resin, 1 part of organic silicon synergistic flame retardant additive, 2 parts of organic silicon toughening agent, 4 parts of phosphorus-containing silicon flame retardant, 0.3 parts of sulfonate flame retardant, 2 parts of zinc borate, 1 part of triphenyl boric acid, 0.4 parts of octamolybdenum, 2 parts of phosphate flame retardant, 0.3 parts of anti-dripping agent, 0.3 parts of antioxidant, 0.2 parts of ultraviolet absorber and 0.5 parts of lubricant.
[0104] The PC resin is preferably Shandong Lihua Yiweiyuan WY-111BR; the ABS resin is selected from BASF's GP-22.
[0105] The organosilicon synergistic flame retardant additive is phenyl silsesquioxane, preferably SIFR-907 provided by QuanSheng Polycarbonate Technology Co., Ltd.
[0106] The sulfonate flame retardant is selected from Quansheng KKS-A2.
[0107] The organosilicon toughening agent is selected from USI3305 of Quansheng.
[0108] The anti-dripping agent is selected from KT-P205 of Quansheng.
[0109] The phosphate flame retardant is PX220.
[0110] The ultraviolet absorber is preferably ultraviolet absorber UV-329; the lubricant is preferably PETS lubricant.
[0111] The antioxidant is composed of a primary antioxidant and an auxiliary antioxidant in a ratio of 1:1. The primary antioxidant is selected from antioxidant 1010; the auxiliary antioxidant is selected from antioxidant 168.
[0112] The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method:
[0113] A1. Dry the PC resin at 120°C until the water content is less than 0.02% and set aside;
[0114] A2. Dry the ABS resin at 85°C until the water content is less than 0.02%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside.
[0115] A3. Add the mixed raw materials into a twin-screw extruder, and obtain a flame-retardant PC / ABS material after extrusion and granulation; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 260 RPM.
[0116] Example 6
[0117] A low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material comprises the following raw materials in parts by weight: 60 parts of PC resin, 30 parts of ABS resin, 1 part of organic silicon synergistic flame retardant additive, 2 parts of organic silicon toughening agent, 5 parts of phosphorus-containing silicon flame retardant, 0.3 parts of sulfonate flame retardant, 2 parts of zinc borate, 1 part of triphenyl boric acid, 0.3 parts of octamolybdenum, 2 parts of phosphate flame retardant, 0.3 parts of anti-dripping agent, 0.3 parts of antioxidant, 0.2 parts of ultraviolet absorber and 0.5 parts of lubricant.
[0118] The PC resin is preferably Shandong Lihua Yiweiyuan WY-111BR; the ABS resin is selected from BASF's GP-22.
[0119] The organosilicon synergistic flame retardant additive is phenyl silsesquioxane, preferably SIFR-908 provided by QuanSheng Polycarbonate Technology Co., Ltd.
[0120] The sulfonate flame retardant is selected from Quansheng KKS-A2.
[0121] The organosilicon toughening agent is selected from USI3305 of Quansheng.
[0122] The anti-dripping agent is selected from KT-P205 of Quansheng.
[0123] The phosphate flame retardant is SPB-100.
[0124] The ultraviolet absorber is preferably ultraviolet absorber UV-329; the lubricant is preferably PETS lubricant.
[0125] The antioxidant is composed of a primary antioxidant and an auxiliary antioxidant in a ratio of 1:1. The primary antioxidant is selected from antioxidant 1010; the auxiliary antioxidant is selected from antioxidant 168.
[0126] The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method:
[0127] A1. Dry the PC resin at 120°C until the water content is less than 0.02% and set aside;
[0128] A2. Dry the ABS resin at 85°C until the water content is less than 0.02%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside.
[0129] A3. Add the mixed raw materials into a twin-screw extruder, and obtain a flame-retardant PC / ABS material after extrusion and granulation; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 260 RPM.
[0130] Example 7
[0131] A low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material comprises the following raw materials in parts by weight: 60 parts of PC resin, 30 parts of ABS resin, 1 part of organic silicon synergistic flame retardant additive, 2 parts of organic silicon toughening agent, 5 parts of phosphorus-containing silicon flame retardant, 0.3 parts of sulfonate flame retardant, 2 parts of zinc borate, 1 part of triphenyl boric acid, 0.4 parts of octamolybdenum, 2 parts of phosphate flame retardant, 0.3 parts of anti-dripping agent, 0.3 parts of antioxidant, 0.2 parts of ultraviolet absorber and 0.5 parts of lubricant.
[0132] The PC resin is preferably 2805 from Covestro; and the ABS resin is GP-22 from BASF.
[0133] The organosilicon synergistic flame retardant additive is phenyl silsesquioxane, preferably SIFR-907 provided by QuanSheng Polycarbonate Technology Co., Ltd.
[0134] The sulfonate flame retardant is selected from Quansheng KKS-A2.
[0135] The organosilicon toughening agent is selected from USI3305 of Quansheng.
[0136] The anti-dripping agent is selected from KT-P205 of Quansheng.
[0137] The phosphate flame retardant is PX200.
[0138] The ultraviolet absorber is preferably ultraviolet absorber UV-329; the lubricant is preferably PETS lubricant.
[0139] The antioxidant is composed of a primary antioxidant and an auxiliary antioxidant in a ratio of 1:1. The primary antioxidant is selected from antioxidant 1010; the auxiliary antioxidant is selected from antioxidant 168.
[0140] The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method:
[0141] A1. Dry the PC resin at 120°C until the water content is less than 0.02% and set aside;
[0142] A2. Dry the ABS resin at 85°C until the water content is less than 0.02%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside.
[0143] A3. Add the mixed raw materials into a twin-screw extruder, and obtain a flame-retardant PC / ABS material after extrusion and granulation; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 260 RPM.
[0144] Example 8
[0145] A low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material comprises the following raw materials in parts by weight: 60 parts of PC resin, 30 parts of ABS resin, 1 part of organic silicon synergistic flame retardant additive, 2 parts of organic silicon toughening agent, 5 parts of phosphorus-containing silicon flame retardant, 0.3 parts of sulfonate flame retardant, 2 parts of zinc borate, 1 part of triphenyl boric acid, 0.4 parts of octamolybdenum, 2 parts of phosphate flame retardant, 0.3 parts of anti-dripping agent, 0.3 parts of antioxidant, 0.2 parts of ultraviolet absorber and 0.5 parts of lubricant.
[0146] The PC resin is preferably 2805 from Covestro; and the ABS resin is GP-22 from BASF.
[0147] The organosilicon synergistic flame retardant additive is phenyl silsesquioxane, preferably SIFR-907 provided by QuanSheng Polycarbonate Technology Co., Ltd.
[0148] The sulfonate flame retardant is selected from Quansheng KKS-A2.
[0149] The organosilicon toughening agent is selected from USI3305 of Quansheng.
[0150] The anti-dripping agent is selected from KT-P205 of Quansheng.
[0151] The phosphate flame retardant is SPB-100.
[0152] The ultraviolet absorber is preferably ultraviolet absorber UV-329; the lubricant is preferably PETS lubricant.
[0153] The antioxidant is composed of a primary antioxidant and an auxiliary antioxidant in a ratio of 1:1. The primary antioxidant is selected from antioxidant 1010; the auxiliary antioxidant is selected from antioxidant 168.
[0154] The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method:
[0155] A1. Dry the PC resin at 120°C until the water content is less than 0.02% and set aside;
[0156] A2. Dry the ABS resin at 85°C until the water content is less than 0.02%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside.
[0157] A3. Add the mixed raw materials into a twin-screw extruder, and obtain a flame-retardant PC / ABS material after extrusion and granulation; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 260 RPM.
[0158] Comparative Examples 1 to 3
[0159] The PC resin was selected from 2805 of Covestro, the ABS resin was selected from GP-22 of BASF, and other additives were tested according to the proportions of the groups listed in Table 1. The process was the same as that of Example 5.
[0160] The PC / ABS alloy halogen-free flame retardant materials obtained in Examples 5 to 8 and Comparative Examples 1 to 3 were injection molded into standard test specimens and tested for performance. The test results are shown in Table 2.
[0161] Test, molding process conditions: nozzle temperature 240℃, temperatures of each zone 220℃, 235℃, 240℃, holding time 6-10s, injection pressure 30-50MPa.
[0162] The test methods for various performances are as follows:
[0163] Tensile strength: tested according to ASTM D638 standard;
[0164] Bending strength: tested according to ASTM D790 standard; Lzod notched impact strength: tested according to ASTM D256 standard; Smoke density: tested according to GB / T 8627-2007 standard; Heat deformation temperature: tested according to ASTM D648 standard;
[0165] Flame retardancy: tested according to UL94 V0 standard.
[0166] Table 1
[0167] materials Comparative Example 1 Comparative Example 2 Comparative Example 3 PC 60.0 60.0 60.0 ABS 30.0 30.0 30.0 SIFR-907 1.0 1.0 1.0 SIFR-908 KKS-A2 0.3 0.3 0.3 PSI-FR 0 5.0 0 Zinc borate 2.0 0 0 Triphenylboronic acid 1.0 0 0 Octa-Molybdenum 0.4 0 0 USI-3305 2.0 2.0 2.0 KT-P205 0.3 0.3 0.3 PX200 BDP 6 5 RDP 5 PX220 2 SPB-100 Antioxidants 0.3 0.3 0.3 UV absorber 0.2 0.2 0.2 Lubricants 0.5 0.5 0.5
[0168] Table 2 Physical properties
[0169]
[0170]
[0171] It can be seen from Table 2 that, compared with Comparative Examples 1-3, the PC / ABS alloy halogen-free flame retardant materials prepared in Examples 5 to 8 have good mechanical properties and flame retardant properties, and also have the advantages of low smoke and high modulus.
[0172] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A method for preparing a phosphorus-silicon flame retardant, characterized in that: The steps include: S1. Add phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double end cap into a mixed system of methanol and water in proportion, stir evenly, add an acidic catalyst, adjust the pH value to 4-6, control the temperature at 0°C to 45°C to react for 8-12h, neutralize, wash, and degas at -0.098MPa, 85°C to obtain an intermediate for standby use; S2. Add DOPO flame retardant in an equal molar ratio to the vinyl in the vinyl double head and DMF in an equal mass ratio to the intermediate to the intermediate obtained in step S1, heat to 60°C to 75°C for 4 to 12 hours, filter, wash and dry to obtain a phosphorus-containing silicon flame retardant.
2. A phosphorus-silicon flame retardant according to claim 1, characterized in that: The phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double head are mixed in a molar ratio of 0.1-3:0.5-4:0.1-0.5; the methanol and water are mixed in a mass ratio of 1:0.8-1.2 to form a mixed system.
3. The method for preparing a phosphorus-silicon flame retardant according to claim 1, characterized in that: The mass ratio of the mixture of phenyltrimethoxysiloxane, methylphenyldimethoxysilane and vinyl double-capped silane to the mixed system of methanol and water is 1:0.8-1.
2.
4. The method for preparing a phosphorus-silicon flame retardant according to claim 1, characterized in that: The phenyl trimethoxysiloxane, methyl phenyl dimethoxy silane and vinyl double end cap are mixed in a molar ratio of 0.1-1:0.5-4:0.1-0.4, and the solid content thereof is 35%-60%.
5. The method for preparing a phosphorus-silicon flame retardant according to claim 1, characterized in that: The acid catalyst is at least one of benzenesulfonic acid, p-toluenesulfonic acid, sulfuric acid, hydrochloric acid, trifluoromethanesulfonic acid, methanesulfonic acid, dodecylbenzenesulfonic acid, phosphoric acid, and strong acid hydrogen salt.
6. A low smoke, high modulus PC / ABS alloy halogen-free flame retardant material, characterized by: The invention comprises the following raw materials in parts by weight: 30-60 parts of PC resin, 5-30 parts of ABS resin, 1-3 parts of organosilicon synergistic flame retardant additive, 1-3 parts of organosilicon toughening agent, 3-5 parts of phosphorus-containing silicon flame retardant according to any one of claims 1 to 5, 0.1-2 parts of sulfonate flame retardant, 1-5 parts of zinc borate, 1-3 parts of triphenyl boric acid, 0.1-0.5 parts of octamolybdenum, 0.5-3 parts of phosphate flame retardant, 0.1-0.5 parts of anti-dripping agent, 0.3-1 parts of antioxidant, 0.2-0.5 parts of ultraviolet absorber and 0.5-1 parts of lubricant; the melt index of the PC resin is 8-12 g / 10 min.
7. The low-smoke, high-modulus PC / ABS alloy halogen-free flame-retardant material according to claim 1, characterized in that: The organosilicon synergistic flame retardant additive is phenyl silsesquioxane.
8. The low-smoke, high-modulus PC / ABS alloy halogen-free flame-retardant material according to claim 1, characterized in that: The phosphate flame retardant is at least one of FCR210, SPB-100, HM1100, PX200 and PX220.
9. The low-smoke, high-modulus PC / ABS alloy halogen-free flame-retardant material according to claim 1, characterized in that: The antioxidant consists of a main antioxidant and an auxiliary antioxidant, wherein the main antioxidant is selected from at least one of antioxidant 1010, antioxidant 1076 and antioxidant MD-697; and the auxiliary antioxidant is selected from at least one of antioxidant 168 and antioxidant 412S.
10. A low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material according to any one of claims 6 to 9, characterized in that: The low-smoke, high-modulus PC / ABS alloy halogen-free flame retardant material is prepared by the following method: A1. Dry the PC resin at 120-130°C until the water content is less than 0.025% and set aside; A2. Dry the ABS resin at 85-90°C until the water content is less than 0.025%. Weigh the other raw materials according to their weight, then mix all the raw materials evenly and set aside. A3. Add the mixed raw materials into a twin-screw extruder, and obtain flame-retardant PC / ABS material after extrusion and granulation; wherein the processing temperature of each zone of the twin-screw extruder is 220-240° C., and the screw speed is 250-300 RPM.
Citation Information
Patent Citations
Hyper-branched phosphorus-containing organic silicon intumescent flame retardant, preparation method and flame-retardant polymer coating composition
CN112625244A
Phosphorus-silicon flame-retardant synergist, ultrathin halogen-free flame-retardant PC / ABS alloy material and preparation method thereof
CN116199938A
Halogen-free phosphorus-containing silicon flame retardant, flame retardant transparent polycarbonate material, and preparation and use thereof
WO2018014443A1
Cited By
Acrylonitrile-styrene-butadiene copolymer material and preparation method thereof
CN119752094A
Fluoride-free environment-friendly flame-retardant PC material and preparation method thereof
CN119752143A
High-temperature-resistant flame-retardant PVC (polyvinyl chloride) material and preparation method thereof
CN120040887A