Silicone rubber emulsion and preparation method thereof
By using a combination of silicone rubber, composite emulsifier and water in the mechanical emulsification method, the problems of poor stability and insufficient heat resistance during the preparation of silicone rubber emulsification are solved, and the preparation of high stability of silicone rubber emulsification under mild conditions is achieved. , suitable for applications of heat-resistant coatings and high-temperature-resistant coatings.
Patent Information
- Application Number
- CN202411071795.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-08
AI Technical Summary
The existing mechanical emulsification method for preparing silicone rubber emulsions has the problem of complex operation, long time, and difficult to obtain high stability emulsions. Moreover, silicone rubber emulsions have limited high and low temperature resistance and cannot be widely used in the field of heat-resistant coatings.
The preparation method containing silicone rubber, composite emulsifier and water is adopted. The composite emulsifier consists of ionic and non-ionic emulsifiers. By combining the type and temperature control of the emulsifier, a stable silicone rubber emulsion can be prepared under mild conditions.
It has achieved the preparation of stable silicone rubber latex in a short time, with good freeze-thaw stability and high environmental protection, and is suitable for applications of heat-resistant coatings and high-temperature-resistant coatings.
Smart Images

Figure CN118909270A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fine chemical preparations, and more specifically to a silicone rubber emulsion and a preparation method thereof. Background Art
[0002] Silicone rubber emulsion is an important organic silicon product and is widely used in industry. Due to its unique performance and characteristics, in addition to being used as a fabric finishing agent in the textile industry, it is also widely used in leather, papermaking, medicine, electronics and electrical, medicine, cosmetics, etc., and its application fields are constantly updated, with great application potential. Therefore, silicone rubber emulsion is also one of the current research hotspots.
[0003] There are two main methods for preparing silicone rubber emulsions, namely, direct emulsion polymerization directly prepared by emulsion polymerization or mechanical emulsification obtained by mixing silicone rubber, emulsifier and water and then stirring at high speed and mechanical emulsification. The emulsifiers used in the preparation of silicone rubber emulsions are mainly divided into anionic emulsifiers, cationic emulsifiers, amphoteric emulsifiers and non-ionic emulsifiers. The silicone rubber emulsion prepared by direct emulsion polymerization has good dispersibility and stability. The stability of silicone rubber emulsion prepared by mechanical emulsification is related to the emulsifier used, emulsification equipment, temperature and silicone rubber content. Generally, the stability of the emulsion prepared is poor, and it is difficult to obtain a stable emulsion with a high molar mass, but the mechanical emulsification method is simpler to operate.
[0004] People have conducted various studies on the preparation of silicone rubber emulsion by mechanical emulsification. For example, a study added silicone rubber polymer, polyether-modified polysiloxane and acidic mixed additive into a container, added emulsifier after thorough mixing, added water and then added stabilizer to obtain a stable silicone rubber emulsion. Although this method can obtain silicone rubber emulsion, it has many disadvantages, such as complicated operation process and long heat preservation time. For example, a study stirred silicone rubber and oily emulsifier to obtain silicone rubber crude emulsion, then mixed aqueous emulsifier, pH adjuster, mechanical stabilizer and soft water, heated and added to silicone rubber crude emulsion to obtain silicone rubber emulsion. Although this method can obtain silicone rubber emulsion, the obtained silicone rubber emulsion must be parked for at least 24 hours, filtered to finally obtain high-temperature silicone rubber emulsion, the entire operation time is long, and it is difficult to obtain silicone rubber emulsion without demulsification and phase separation.
[0005] Therefore, developing a mechanical emulsification method that can obtain silicone rubber emulsion with good stability has become a problem to be solved.
[0006] As mentioned above, silicone rubber emulsion is usually prepared by direct emulsion polymerization or mechanical emulsification of methyl silicone oil / silicone rubber or modified methyl silicone oil / silicone rubber. Although the obtained emulsion has a certain stability, due to the limited high and low temperature resistance of the matrix raw material, the synthesized emulsion is difficult to be used in the fields of heat-resistant coatings and the like. It is known that phenyl silicone rubber can be used for the preparation of heat-resistant coatings or high-temperature resistant paints, but it is currently mainly used in organic solvent systems, so the construction process cannot achieve green environmental protection. The present invention aims to provide a novel method for preparing silicone rubber emulsion, which can be applied to the preparation of phenyl silicone rubber emulsion, so as to solve the problem of limited high and low temperature resistance in the application field of ordinary methyl silicone oil or modified silicone oil emulsion, and at the same time, the preparation and construction process of phenyl silicone rubber coating can be achieved in a green, environmentally friendly, safe and reliable manner. Summary of the invention
[0007] The first aspect of the present invention provides a silicone rubber emulsion, which comprises silicone rubber, a composite emulsifier and water.
[0008] Based on 100 parts by mass of the silicone rubber, the content of the composite emulsifier is 1-10 parts by mass, and the content of water is 100-10000 parts by mass;
[0009] The composite emulsifier comprises a first emulsifier and a second emulsifier, the first emulsifier is an ionic emulsifier or a nonionic emulsifier, the second emulsifier is a nonionic emulsifier, and the weight ratio of the first emulsifier to the second emulsifier is 1:6 to 5:1;
[0010] The ionic emulsifier is selected from one or more of the following: C1-20 alkyl sulfonate, C1-20 alkyl C6-C22 aryl sulfonate, tetra(C1-20 alkyl) ammonium halide, tri(C1-20 alkyl) C6-C22 aryl ammonium halide;
[0011] The nonionic emulsifier is selected from one or more of the following: polyether emulsifier, polyester emulsifier, polyether-polyester emulsifier.
[0012] A second aspect of the present invention provides a method for preparing a silicone rubber emulsion, characterized in that silicone rubber, a composite emulsifier and water are mixed;
[0013] The composite emulsifier comprises a first emulsifier and a second emulsifier, the first emulsifier is an ionic emulsifier or a nonionic emulsifier, the second emulsifier is a nonionic emulsifier, and the weight ratio of the first emulsifier to the second emulsifier is 1:6 to 5:1;
[0014] The ionic emulsifier is selected from one or more of the following: C1-20 alkyl sulfonate, C1-20 alkyl C6-C22 aryl sulfonate, tetra(C1-20 alkyl) ammonium halide, tri(C1-20 alkyl) C6-C22 aryl ammonium halide;
[0015] The nonionic emulsifier is selected from one or more of the following: polyether emulsifier, polyester emulsifier, polyether-polyester emulsifier.
[0016] In a preferred embodiment, the silicone rubber is a copolymer silicone rubber.
[0017] In a preferred embodiment, the copolymeric silicone rubber comprises a first copolymeric unit and a second copolymeric unit.
[0018] In a preferred embodiment, the first copolymeric unit is of the formula "-SiOR 1 R 2 -”, where R 1 and R 2 are independently selected from: C1-20 alkyl, C3-C16 cycloalkyl, C1-C20 alkoxy, C2-C18 alkenyl, halogenated C1-C20 alkyl, C6-C16 aryl, and the proviso that R 1 and R 2 At least one of them is a C6-C16 aryl group.
[0019] In a preferred embodiment, the second copolymeric unit is of the formula "-SiOR 3 R 4 -”, where R 3 and R 4 Each is independently selected from the group consisting of: C1-20 alkyl, C3-C16 cycloalkyl, C1-C20 alkoxy, C2-C18 alkenyl, and halogenated C1-C20 alkyl.
[0020] In a preferred embodiment, the molar ratio of the first copolymerization unit to the second copolymerization unit is 1:100-100:1.
[0021] In a preferred embodiment, the number average molecular weight of the copolymer silicone rubber is 2500-800,000.
[0022] In a preferred embodiment, the method comprises the following steps in sequence:
[0023] Step I: mixing the silicone rubber and the composite emulsifier to obtain a first mixture;
[0024] Step II: adding water to the first mixture to obtain a silicone rubber emulsion.
[0025] In a preferred embodiment, the method comprises the following steps in sequence:
[0026] Step I': mixing water with the composite emulsifier to obtain an emulsifier liquid material;
[0027] Step II': adding silicone rubber to the emulsifier liquid material to obtain silicone rubber emulsion.
[0028] In a preferred embodiment, the step I is carried out at a temperature of 0°C-100°C.
[0029] In a preferred embodiment, the step II is carried out at a temperature of 0°C-100°C.
[0030] In a preferred embodiment, the step I' is carried out at a temperature of 0°C-100°C.
[0031] In a preferred embodiment, the step II' is carried out at a temperature of 0°C-100°C.
[0032] In a preferred embodiment, the duration of step I is 1 min-2 h.
[0033] In a preferred embodiment, the duration of step II' is 1 min-5 h;
[0034] In a preferred embodiment, the duration of step I' is 1 min-2 h.
[0035] In a preferred embodiment, the duration of step II' is 1 min-5 h.
[0036] In a preferred embodiment, the ionic emulsifier is selected from: sodium dodecylbenzene sulfonate (SDBS), dodecyldimethylbenzylammonium bromide, dodecyltrimethylammonium chloride.
[0037] In a preferred embodiment, the nonionic emulsifier is selected from: octadecyl alcohol polyoxyethylene ether (Perchlorate O), octylphenyl polyoxyethylene ether (Triton), lauryl alcohol polyoxyethylene ether (Brij35), sorbitan oleate polyoxyethylene ether (Tween80), and sorbitan monostearate.
[0038] In a preferred embodiment, the mass ratio of the composite emulsifier to the silicone rubber is 0.1:100 to 30:100.
[0039] The third aspect of the present invention provides a coating, which is prepared from the silicone rubber emulsion of the present invention.
[0040] A fourth aspect of the present invention provides a product comprising at least one coating layer, wherein the coating layer is formed from the above-mentioned coating material.
[0041] Compared with the prior art, the present invention has the following advantages:
[0042] 1. The present invention can prepare a stable emulsion under mild conditions by adjusting the type of emulsifier and regulating the temperature and the content of silicone rubber.
[0043] 2. The preparation process of the present invention does not involve complex operating environments such as high pressure, high speed, and long-term stirring. The preparation process time is controlled within 5 hours, which can reduce energy consumption and has lower requirements for equipment.
[0044] 3. The silicone rubber emulsion prepared by the present invention can be stored for a long time without stratification and has good freeze-thaw stability.
[0045] 4. The chemical substances used in the preparation process of the silicone rubber emulsion of the present invention are all non-toxic or low-toxic, and have good environmental protection.
[0046] The silicone rubber emulsion of the present invention can be applied to the field of thermal management of materials in complex environments such as heat-resistant coatings, high-temperature-resistant coatings, radiation-resistant and ablation-resistant materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 shows the reaction equipment used in the embodiments of the present invention;
[0048] Figure 2 The emulsion product prepared in the example of the present invention is shown. DETAILED DESCRIPTION
[0049] The "range" disclosed herein is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In this application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0050] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.
[0051] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0052] In the present application, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0053] In this application, unless otherwise specified, the terms "include" and "comprising" mentioned herein may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0054] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and "several" in "one or several" means two or more.
[0055] In the description herein, unless otherwise specified, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0056] Herein, unless otherwise specified, percentage (%) or part refers to percentage by weight or part by weight relative to the composition.
[0057] Herein, if there is no contrary description, the sum of the contents of the various components in the composition is 100%.
[0058] In this context, unless otherwise specified, "a combination thereof" means a multi-component mixture of the elements described, for example a mixture of two, three, four and up to the maximum possible multi-component mixture.
[0059] If not specifically stated, the terms "a" or "an" used in the present specification means "at least one".
[0060] The silicone rubber emulsion of the present invention comprises silicone rubber, a composite emulsifier and water.
[0061] The silicone rubber contained in the silicone rubber emulsion of the present invention is preferably a copolymer silicone rubber, which preferably comprises a first copolymerization unit and a second copolymerization unit.
[0062] In a preferred embodiment, the first copolymeric unit is of the formula "-SiOR 1 R 2 -”. In the formula “-SiOR 1 R 2 -" in the first copolymerization unit, the R 1 and R 2 According to one embodiment of the present application, the first copolymer unit can be obtained by polymerization (e.g., polycondensation) of the corresponding first copolymer monomer, for example, the corresponding first copolymer monomer can have a structure shown in the following formula: "SiR 1 R 2 (OH) 2 ”.
[0063] In a preferred embodiment, R 1 and R 2 are independently selected from: C1-20 alkyl, C3-C16 cycloalkyl, C1-C20 alkoxy, C2-C18 alkenyl, halogenated C1-C20 alkyl, C6-C16 aryl, and the proviso that R 1 and R 2 In a preferred embodiment, at least one of R 1 and R 2 All are C6-C16 aryl groups, preferably all are phenyl groups or phenyl groups substituted with one or more C1-C6 alkyl groups, and more preferably all are phenyl groups.
[0064] In a preferred embodiment, the second copolymeric unit is of the formula "-SiOR 3 R 4 -”. The formula is “-SiOR 3 R 4 -" in the second copolymerization unit, the R 3 and R 4 According to one embodiment of the present application, the second copolymer unit can be obtained by polymerization (e.g., polycondensation) of a corresponding second comonomer, for example, the corresponding second comonomer can have a structure shown in the following formula: "SiR3 R 4 (OH) 2 ”.
[0065] In a preferred embodiment, R 3 and R 4 Each of the following is independently selected from: C1-20 alkyl, C3-C16 cycloalkyl, C1-C20 alkoxy, C2-C18 alkenyl, halogenated C1-C20 alkyl. 3 and R 4 All are C1-20 alkyl, preferably all are C1-6 alkyl, more preferably all are methyl.
[0066] In a preferred embodiment, the structure of the silicone rubber is shown in the following formula I:
[0067]
[0068] Wherein, m is an integer from 1 to 3000, and n is an integer from 1 to 3000.
[0069] In a preferred embodiment, the molar ratio of the first copolymerization unit to the second copolymerization unit is 1:100-100:1, preferably 1:50-50:1, and more preferably 1:20-20:1.
[0070] In a preferred embodiment, the dynamic viscosity (25° C.) of the silicone rubber may be 1000-20000 cP, preferably 3000-10000 cP.
[0071] In the present invention, dynamic viscosity, also known as absolute viscosity or simple viscosity, is defined as the ratio of stress to strain rate at a certain temperature, which is numerically equal to the area of 1m 2 When two plates 1m apart move relative to each other at a speed of 1m / s, the internal friction generated by the interaction of the fluid between them is expressed in N·s / m. 2 , that is, Pa·s.
[0072] In a preferred embodiment, the silicone rubber is a silicone rubber represented by formula I, and based on the molar amount of all copolymerized units in the silicone rubber, the molar percentage of the copolymerized units containing phenyl in the silicone rubber may be 1 mol %-30 mol %, preferably 3 mol %-15 mol %.
[0073] In a preferred embodiment, the number average molecular weight of the copolymer silicone rubber is 2500-800,000, for example, 3000-500000, or 4000-200000, or 5000-100000, or 6000-80000, or 8000-50000, or 10000-30000, or within the numerical range obtained by combining any two of the above end values.
[0074] The silicone rubber emulsion of the present invention comprises a composite emulsifier, which comprises two or more rubber emulsifiers.
[0075] In a preferred embodiment, the composite emulsifier of the present invention comprises a first emulsifier and a second emulsifier. The first emulsifier is an ionic emulsifier or a nonionic emulsifier, and the second emulsifier is a nonionic emulsifier.
[0076] The ionic emulsifier is selected from one or more of the following: C1-20 alkyl sulfonate, C1-20 alkyl C6-C22 aryl sulfonate, tetra(C1-20 alkyl) ammonium halide, tri(C1-20 alkyl) C6-C22 aryl ammonium halide. The sulfonate is preferably benzene sulfonate. The ammonium halide is preferably ammonium chloride or ammonium bromide.
[0077] The nonionic emulsifier is selected from one or more of the following: polyether emulsifier, polyester emulsifier, polyether-polyester emulsifier.
[0078] In a preferred embodiment, the weight ratio of the first emulsifier to the second emulsifier is 1:6 to 5:1, preferably 1:3 to 3:1, for example 1:2 to 2:1, or 1:1, or within the numerical range obtained by combining any two of the above ratios.
[0079] According to a preferred embodiment of the present application, the ionic emulsifier is selected from one or more of the following: sodium dodecylbenzene sulfonate (SDBS), dodecyldimethylbenzylammonium bromide, dodecyltrimethylammonium chloride.
[0080] According to another preferred embodiment of the present application, the nonionic emulsifier is selected from one or more of the following: octadecyl alcohol polyoxyethylene ether (pegylated O), octylphenyl polyoxyethylene ether (Triton), lauryl alcohol polyoxyethylene ether (Brij35), sorbitan oleate polyoxyethylene ether (Tween80), and sorbitan monostearate.
[0081] According to an exemplary embodiment of the present application, the composite emulsifier consists of sodium dodecylbenzene sulfonate (SDBS) and polyoxyethylene lauryl alcohol ether (Brij35).
[0082] According to an exemplary embodiment of the present application, the composite emulsifier consists of sorbitan oleate polyoxyethylene ether (Tween 80) and lauryl alcohol polyoxyethylene ether (Brij 35).
[0083] According to an exemplary embodiment of the present application, the composite emulsifier consists of dodecyl dimethyl benzyl ammonium bromide and sorbitan oleate polyoxyethylene ether (Tween 80).
[0084] According to an exemplary embodiment of the present application, the composite emulsifier consists of dodecyldimethylbenzylammonium bromide and sorbitan monostearate.
[0085] According to a specific embodiment of the present application, the composite emulsifier is a combination of sodium dodecylbenzene sulfonate (SDBS) and lauryl alcohol polyoxyethylene ether (Brij35), and the weight ratio of the two is 1:1 to 1:2. According to another specific embodiment of the present application, the composite emulsifier is a combination of sorbitan oleate polyoxyethylene ether (Tween80) and lauryl alcohol polyoxyethylene ether (Brij35), and the weight ratio of the two is 1:1 to 2:3. According to another specific embodiment of the present application, the composite emulsifier is a combination of dodecyl dimethyl benzyl ammonium bromide and sorbitan oleate polyoxyethylene ether (Tween80), and the weight ratio of the two is 1:1 to 3:4. According to another specific embodiment of the present application, the composite emulsifier is a combination of dodecyl dimethyl benzyl ammonium bromide and sorbitan monostearate, and the weight ratio of the two is 2:1 to 1:1.
[0086] In a preferred embodiment, based on 100 parts by mass of the silicone rubber, the content of the composite emulsifier may be 0.1-30 parts by mass, preferably 1-10 parts by mass, preferably 2-10 parts by mass, and more preferably 4-8 parts by mass.
[0087] The silicone rubber emulsion of the present invention contains water, which may be deionized water.
[0088] In a preferred embodiment, based on 100 parts by mass of the silicone rubber, the water content is 100-10000 parts by mass, preferably 100-1000 parts by mass, and more preferably 100-500 parts by mass.
[0089] The preparation method of the present invention mixes silicone rubber, a composite emulsifier and water to prepare a silicone rubber emulsion. The mixing can be performed in steps or in one step, but preferably in steps.
[0090] In a preferred embodiment, the method comprises the following steps in sequence:
[0091] Step I: mixing the silicone rubber and the composite emulsifier to obtain a first mixture;
[0092] Step II: adding water to the first mixture to obtain a silicone rubber emulsion.
[0093] In step I, the mixing temperature may be 0°C-100°C, preferably 20°C-80°C, more preferably 20°C-50°C.
[0094] In step I, the mixing speed may be 100-2000 r / min, preferably 500-1500 r / min, more preferably 800-1200 r / min.
[0095] In step I, the mixing time may be 1 min-2 h, preferably 5 min-1.5 h, more preferably 10 min-1 h.
[0096] In step I, based on 100 parts by mass of the silicone rubber, the content of the composite emulsifier may be 0.1-30 parts by mass, preferably 1-10 parts by mass, preferably 2-10 parts by mass, and more preferably 4-8 parts by mass.
[0097] In step II, the mixing time may be 1 min to 5 h, preferably 5 min to 4 h, more preferably 10 min to 3 h.
[0098] In step II, the mixing speed is preferably greater than that in step I. In a preferred embodiment, in step II, the mixing speed may be 500-10000 r / min, preferably 1000-5000 r / min, more preferably 1500-3500 r / min.
[0099] In step II, the water may be deionized water. Based on 100 parts by mass of the silicone rubber, the content of the water is 100-10000 parts by mass, preferably 100-1000 parts by mass, and more preferably 100-500 parts by mass. The water may be added all at once or in batches.
[0100] In a preferred embodiment, the method comprises the following steps in sequence:
[0101] Step I': mixing water with the composite emulsifier to obtain an emulsifier liquid material;
[0102] Step II': adding silicone rubber to the emulsifier liquid material to obtain silicone rubber emulsion.
[0103] In step I', the mixing temperature may be 0°C-100°C, preferably 20°C-80°C, more preferably 20°C-50°C.
[0104] In step I', the mixing rotation speed may be 100-2000 r / min, preferably 500-1500 r / min, more preferably 800-1200 r / min.
[0105] In step I', the mixing time may be 1 min to 2 h, preferably 5 min to 1.5 h, more preferably 10 min to 1 h.
[0106] In step I', the water may be deionized water. Based on 100 parts by mass of the silicone rubber, the water content is 100-10000 parts by mass, preferably 100-1000 parts by mass, and more preferably 100-500 parts by mass. The water may be added all at once or in batches.
[0107] In step I', based on 100 parts by mass of the silicone rubber, the content of the composite emulsifier may be 0.1-30 parts by mass, preferably 1-10 parts by mass, preferably 2-10 parts by mass, and more preferably 4-8 parts by mass.
[0108] In step II', the mixing time may be 1 min to 5 h, preferably 5 min to 4 h, more preferably 10 min to 3 h.
[0109] In step II', the mixing speed is preferably greater than that in step I'. In a preferred embodiment, in step II', the mixing speed may be 500-10000 r / min, preferably 1000-5000 r / min, more preferably 1500-3500 r / min.
[0110] Example
[0111] In the following examples, the inventors prepared silicone rubber emulsion samples and evaluated their physical stability properties.
[0112] The phenyl silicone rubber used in the embodiment is produced by Shanghai Resin Factory, and the number average molecular weight is 2000-6000. The emulsifiers SDBS and sorbitan monostearate are purchased from Greagent, Brij35, Tween80 and dodecyl dimethyl benzyl ammonium bromide are purchased from Adamas, and octadecyl dimethyl benzyl ammonium chloride is purchased from Dr. E. The water used is deionized water.
[0113] Example 1
[0114] like Figure 1As shown, 100 g of silicone rubber (dynamic viscosity at 25° C.: 10000 cP, phenyl content 15 mol%) and 8 g of composite emulsifier (SDBS: Brij35=1:2, weight ratio) were added to a 1000 ml stainless steel reactor, and mechanical stirring was performed at a temperature of 40° C. with a stirring speed of 1000 r / min. The mixture was stirred for 20 min to mix evenly to obtain a mixture.
[0115] Then, the stirring speed was increased to 1500 r / min, 50 g of deionized water was dripped into the above mixture at a rate of 10 g / min, and stirred for 30 min. The stirring speed was increased to 2200 r / min again, 200 g of deionized water was quickly poured in, stirred and kept warm at 40°C for 60 min.
[0116] Finally, the stirring speed was reduced to 1000 r / min, and the mixture was stirred and kept at 40°C for 60 min to obtain a silicone rubber emulsion. Figure 2 shown.
[0117] The obtained silicone rubber emulsion was evaluated.
[0118] First, the obtained silicone rubber emulsion was left to stand at room temperature for 24 hours to observe whether it was separated into layers. As a result, no separation of the obtained silicone rubber emulsion was observed.
[0119] Secondly, the obtained silicone rubber emulsion was placed in a refrigerator and frozen at -20°C, then taken out and allowed to stand at 25°C until it was completely melted. The above operation was repeated 3 times, and the results were observed. No demulsification or phase separation of the obtained silicone rubber emulsion was observed.
[0120] Example 2
[0121] In a 1000 ml stainless steel reactor, 100 g of phenyl silicone rubber (dynamic viscosity at 25° C.: 4000 cP, phenyl content 8 mol%) and 4 g of emulsifier (Tween80: Brij35=2:3, weight ratio) were added, and mechanical stirring was performed at a temperature of 40° C. and a stirring speed of 1200 r / min. Stirring was performed for 20 min to mix evenly to obtain a mixture.
[0122] Then, the stirring speed was increased to 3200 r / min, 400 g of deionized water was quickly poured in, and stirred for 15 min.
[0123] Finally, the stirring speed was reduced to 1000 r / min and the mixture was stirred for 180 min until it became uniform, thereby obtaining the silicone rubber emulsion.
[0124] The obtained silicone rubber emulsion was evaluated.
[0125] First, the obtained silicone rubber emulsion was left to stand at room temperature for 24 hours to observe whether it was separated into layers. As a result, no separation of the obtained silicone rubber emulsion was observed.
[0126] Secondly, the obtained silicone rubber emulsion was placed in a refrigerator and frozen at -20°C, then taken out and allowed to stand at 25°C until it was completely melted. The above operation was repeated 5 times, and the results were observed. No demulsification or phase separation of the obtained silicone rubber emulsion was observed.
[0127] Example 3
[0128] In a 1000 ml stainless steel reactor, 100 g of phenyl silicone rubber (dynamic viscosity at 25° C.: 8000 cP, phenyl content 10 mol%) and 5 g of emulsifier (dodecyl dimethyl benzyl ammonium bromide: Tween 80 = 1:1, weight ratio) were added, and mechanical stirring was performed at a temperature of 50° C. and a stirring speed of 800 r / min. The mixture was stirred for 20 min to mix evenly to obtain a mixture.
[0129] Then, the stirring speed was increased to 3000 r / min, and 200 g of deionized water was dripped into the above mixture at a rate of 20 g / min, and stirred for 30 min.
[0130] Finally, the stirring speed was reduced to 1000 r / min, and the mixture was stirred and kept at 50° C. for 120 min to obtain the silicone rubber emulsion.
[0131] The obtained silicone rubber emulsion was evaluated.
[0132] First, the obtained silicone rubber emulsion was left to stand at room temperature for 24 hours to observe whether it was separated into layers. As a result, no separation of the obtained silicone rubber emulsion was observed.
[0133] Secondly, the obtained silicone rubber emulsion was placed in a refrigerator and frozen at -20°C, then taken out and allowed to stand at 25°C until it was completely melted. The above operation was repeated 5 times, and the results were observed. No demulsification or phase separation of the obtained silicone rubber emulsion was observed.
[0134] Example 4
[0135] 300 g of deionized water and 5 g of an emulsifier (dodecyl dimethyl benzyl ammonium bromide: sorbitan monostearate = 2:1, weight ratio) were added to a 1000 ml stainless steel reactor, and mechanical stirring was performed at a temperature of 50° C. and a stirring speed of 1000 r / min. The mixture was stirred for 20 min to mix evenly to obtain a mixture.
[0136] Then, the stirring speed was increased to 3000 r / min, and 100 g of silicone rubber (dynamic viscosity at 25° C.: 8000 cP, phenyl content 10 mol %) was uniformly added to the above mixture at a rate of 2 g / min, and stirred for 120 min.
[0137] Finally, the stirring speed was reduced to 1000 r / min, and the mixture was stirred and kept at 50° C. for 60 min to obtain the silicone rubber emulsion.
[0138] The obtained silicone rubber emulsion was evaluated.
[0139] First, the obtained silicone rubber emulsion was left to stand at room temperature for 24 hours to observe whether it was separated into layers. As a result, no separation of the obtained silicone rubber emulsion was observed.
[0140] Secondly, the obtained silicone rubber emulsion was placed in a refrigerator and frozen at -20°C, then taken out and allowed to stand at 25°C until it was completely melted. The above operation was repeated 5 times, and the results were observed. No demulsification or phase separation of the obtained silicone rubber emulsion was observed.
[0141] Comparative Example 1
[0142] 100 g of silicone rubber (dynamic viscosity at 25° C.: 10,000 cP, phenyl content 15 mol%) and 8 g of octadecyldimethylbenzyl ammonium chloride were added to a 1000 ml stainless steel reactor, and mechanical stirring was performed at a temperature of 40° C. and a stirring speed of 1000 r / min. Stirring was performed for 20 minutes to mix uniformly to obtain a mixture.
[0143] Then, the stirring speed was increased to 1500 r / min, 50 g of deionized water was dripped into the above mixture at a rate of 10 g / min, and stirred for 30 min. The stirring speed was increased to 2200 r / min again, 200 g of deionized water was quickly poured in, stirred and kept warm at 40°C for 60 min.
[0144] Finally, the stirring speed was reduced to 1000 r / min, and the mixture was stirred and kept at 40° C. for 60 min to obtain the silicone rubber emulsion.
[0145] The obtained silicone rubber emulsion was evaluated.
[0146] First, the obtained silicone rubber emulsion was left to stand at room temperature for 24 hours, and whether it was separated into layers was observed after standing. As a result, it was observed that the obtained silicone rubber emulsion was separated into layers.
[0147] Secondly, the obtained silicone rubber emulsion was placed in a refrigerator and frozen at -20°C, then taken out and allowed to stand at 25°C until it was completely melted. The above operation was repeated 3 times, and the results were observed. It was observed that the obtained silicone rubber emulsion was demulsified and phase separated.
[0148] Comparative Example 2
[0149] 100 g of phenyl silicone rubber (dynamic viscosity at 25° C.: 8000 cP, phenyl content 10 mol%) and 8 g of sodium dodecylbenzene sulfonate were added to a 1000 ml stainless steel reactor, and mechanical stirring was performed at a temperature of 50° C. and a stirring speed of 800 r / min. Stirring was performed for 20 min to mix them evenly to obtain a mixture.
[0150] Then, the stirring speed was increased to 3000 r / min, and 200 g of deionized water was dripped into the above mixture at a rate of 20 g / min, and stirred for 30 min.
[0151] Finally, the stirring speed was reduced to 1000 r / min, and the mixture was stirred and kept at 50° C. for 120 min to obtain the silicone rubber emulsion.
[0152] The obtained silicone rubber emulsion was evaluated.
[0153] First, the obtained silicone rubber emulsion was left to stand at room temperature for 24 hours, and whether it was separated into layers was observed after standing. As a result, it was observed that the obtained silicone rubber emulsion was separated into layers.
[0154] Secondly, the obtained silicone rubber emulsion was placed in a refrigerator and frozen at -20°C, then taken out and allowed to stand at 25°C until it was completely melted. The above operation was repeated 5 times, and the results were observed. It was observed that the obtained silicone rubber emulsion was demulsified and phase separated.
[0155] Comparative Example 3
[0156] In a 1000 ml stainless steel reactor, 100 g of silicone rubber (dynamic viscosity at 25° C.: 10000 cP, phenyl content 15 mol%) and 8 g of a composite emulsifier (sodium dodecylbenzenesulfonate: dodecyldimethylbenzylammonium bromide = 1:2, weight ratio) were added, and mechanical stirring was performed at a temperature of 40° C. and a stirring speed of 1000 r / min. The mixture was stirred for 20 min to mix evenly to obtain a mixture.
[0157] Then, the stirring speed was increased to 1500 r / min, 50 g of deionized water was dripped into the above mixture at a rate of 10 g / min, and stirred for 30 min. The stirring speed was increased to 2200 r / min again, 200 g of deionized water was quickly poured in, stirred and kept warm at 40°C for 60 min.
[0158] Finally, the stirring speed was reduced to 1000 r / min, and the mixture was stirred and kept at 40° C. for 60 min to obtain the silicone rubber emulsion.
[0159] The obtained silicone rubber emulsion was evaluated.
[0160] First, the obtained silicone rubber emulsion was left to stand at room temperature for 24 hours, and whether it was separated into layers was observed after standing. As a result, it was observed that the obtained silicone rubber emulsion was separated into layers.
[0161] Secondly, the obtained silicone rubber emulsion was placed in a refrigerator and frozen at -20°C, then taken out and allowed to stand at 25°C until it was completely melted. The above operation was repeated 3 times, and the results were observed. It was observed that the obtained silicone rubber emulsion was demulsified and phase separated.
Claims
1. A method for preparing a silicone rubber emulsion, characterized in that: The method includes: Mix silicone rubber, composite emulsifier and water; The composite emulsifier comprises a first emulsifier and a second emulsifier, the first emulsifier is an ionic emulsifier or a nonionic emulsifier, the second emulsifier is a nonionic emulsifier, and the weight ratio of the first emulsifier to the second emulsifier is 1:6 to 5:1; The ionic emulsifier is selected from one or more of the following: C1-20 alkyl sulfonate, C1-20 alkyl C6-C22 aryl sulfonate, tetra(C1-20 alkyl) ammonium halide, tri(C1-20 alkyl) C6-C22 aryl ammonium halide; The nonionic emulsifier is selected from one or more of the following: polyether emulsifier, polyester emulsifier, polyether-polyester emulsifier.
2. The method according to claim 1, characterized in that The silicone rubber is a copolymer silicone rubber; The copolymer silicone rubber comprises a first copolymer unit and a second copolymer unit, wherein the first copolymer unit is represented by the formula -SiOR1R2-, wherein R1 and R2 are independently selected from: C1-20 alkyl, C3-C16 cycloalkyl, C1-C20 alkoxy, C2-C18 alkenyl, halogenated C1-C20 alkyl, C6-C16 aryl, and the premise is that at least one of R1 and R2 is C6-C16 aryl; The second copolymer unit is represented by the formula -SiOR3R4-, wherein R3 and R4 are independently selected from: C1-20 alkyl, C3-C16 cycloalkyl, C1-C20 alkoxy, C2-C18 alkenyl, halogenated C1-C20 alkyl, The molar ratio of the first copolymerization unit to the second copolymerization unit is 1:100-100:1, and the number average molecular weight of the copolymer silicone rubber is 2500-800,000.
3. The method according to claim 1 or 2, characterized in that The method comprises the following steps in sequence: Step I: mixing the silicone rubber and the composite emulsifier to obtain a first mixture; Step II: adding water to the first mixture to obtain a silicone rubber emulsion; or Step I': mixing water with the composite emulsifier to obtain an emulsifier liquid material; Step II': adding silicone rubber to the emulsifier liquid material to obtain silicone rubber emulsion.
4. The method according to claim 3, characterized in that The step I, step II, step I' and step II' are all carried out at a temperature of 0°C-100°C.
5. The method according to any one of claims 1 to 4, characterized in that The duration of step I is 1 min-2 h, and the duration of step II' is 1 min-5 h; The duration of step I' is 1 min-2 h, and the duration of step II' is 1 min-5 h.
6. The method according to claim 1, characterized in that The ionic emulsifier is selected from sodium dodecylbenzene sulfonate (SDBS), dodecyl dimethyl benzyl ammonium bromide, dodecyl trimethyl ammonium chloride, The nonionic emulsifier is selected from: octadecyl alcohol polyoxyethylene ether (pegylated O), octylphenyl polyoxyethylene ether (Triton), lauryl alcohol polyoxyethylene ether (Brij35), sorbitan oleate polyoxyethylene ether (Tween80), and sorbitan monostearate.
7. The method according to claim 1, characterized in that The mass ratio of the composite emulsifier to the silicone rubber is 0.1:100 to 30:
100.
8. A silicone rubber emulsion comprising silicone rubber, a composite emulsifier and water, Based on 100 parts by mass of the silicone rubber, the content of the composite emulsifier is 1-10 parts by mass, and the content of water is 100-10000 parts by mass; The composite emulsifier comprises a first emulsifier and a second emulsifier, the first emulsifier is an ionic emulsifier or a nonionic emulsifier, the second emulsifier is a nonionic emulsifier, and the weight ratio of the first emulsifier to the second emulsifier is 1:6 to 5:1; The ionic emulsifier is selected from one or more of the following: C1-20 alkyl sulfonate, C1-20 alkyl C6-C22 aryl sulfonate, tetra(C1-20 alkyl) ammonium halide, tri(C1-20 alkyl) C6-C22 aryl ammonium halide; The nonionic emulsifier is selected from one or more of the following: polyether emulsifier, polyester emulsifier, polyether-polyester emulsifier.
9. The silicone rubber emulsion according to claim 8, which is prepared by the method according to any one of claims 1 to 7.