High-temperature-resistant polyimide aerogel composite material as well as preparation method and application thereof
By using unidirectional vacuum impregnation composite and CO2 supercritical fluid drying in polyimide aerogel, the performance matching problem of polyimide aerogel in the aerospace field is solved, and high performance resistance is achieved High temperature and low density characteristics meet the demand for high-performance thermal protection materials in the aerospace field.
Patent Information
- Application Number
- CN202411274380.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The existing polyimide aerogel materials are difficult to meet the performance requirements of high-performance organic thermal protection materials in the aerospace field, especially in the matching of lightweight, high-strength, ultra-low normal temperature and pressure thermal conductivity and excellent high-temperature resistance. problem.
Using a one-way vacuum impregnation composite method of aerogel and fiber preform, the enhanced polyimide sol is formed by adding metal oxide organic precursors or non-metal oxide organic precursors and crosslinking agents, and unidirectional Vacuum impregnation composite and CO2 supercritical fluid drying were prepared to produce high-temperature resistant polyimide aerogel composite.
Improve the tolerance temperature and mechanical strength of polyimide aerogel, achieving high-performance applications in 420℃ environment, with a thermal decomposition temperature of 700℃, and a thermal conductivity of normal temperature and pressure between 0.020 and 0.032W/(m ·K) The density is 0.09~0.20g/cm3, meeting the lightweight and high-strength needs in the temperature range of 320~700℃.
Smart Images

Figure CN118909301A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high-performance thermal protection materials in the field of aerospace, and in particular to a high-temperature resistant polyimide aerogel composite material and a preparation method and application thereof. Background Art
[0002] Thermal protection materials play an indispensable role in the aerospace field. Lightweight, high-strength, high-performance organic thermal protection materials are of great significance to the lightweight load, improved carrying capacity, increased flight speed and extended range of aircraft. With the high-level development of aerospace technology, traditional thermal protection materials are difficult to adapt to the performance requirements of the thermal protection system of current aircraft due to various defects. Therefore, it is urgent to develop new high-performance organic thermal protection materials with lightweight, high strength and high temperature resistance. Aerogel is the lightest known solid material with the lowest thermal conductivity, and is known as a super thermal insulation material. Due to its excellent temperature resistance and thermal insulation performance, it has attracted much attention in the aerospace field. Inorganic aerogels represented by SiO2 are widely used in many fields, but their brittleness, fragility and insufficient thermal stability limit their practical application in the aerospace field. In contrast, organic polymer aerogel materials have better flexibility, mechanical properties and thermal stability, and show great application potential in the aerospace field. Among them, polyimide aerogel has attracted much attention due to its excellent comprehensive performance and excellent application performance in the aerospace field. Zhang et al. reported a polyimide aerogel material that can withstand 200°C, with a thermal decomposition temperature of 504°C. Although it has good mechanical properties, the thermal stability of the polyimide aerogel is insufficient. After cycling from 150°C to -50°C, the elastic modulus decreased by 9%. At the same time, its dimensional stability is insufficient: at 200°C and 2400s, the shrinkage rate reached more than 9.7% [ACS Applied Nano Materials. 2023, 6, 7269-7279]. Zhang et al. reported a polyimide aerogel with better comprehensive performance. A high-temperature resistant polyimide aerogel was prepared by hybridizing Al2O3 with polyimide aerogel. 2,4,6-triaminopyrimidine was introduced as a cross-linking agent to enhance the three-dimensional network skeleton of the polyimide aerogel. The prepared polyimide aerogel has a density of 0.128g / cm 3, the compressive stress under 3% compressive strain conditions is 0.417MPa, the minimum thermal conductivity is 0.0235W / (m·K), and it can be used at a high temperature of up to 250°C. After 5 high-temperature cycles (250°C, 2400s), the mass change rate of the aerogel is ≤0.3%, the shrinkage rate is ≤2.53%, the thermal conductivity change is ≤3%, and the volume density is almost unchanged [ACS AppliedNano Materials.2023,6,15925-15936]. Zhang et al. reported an ultra-light aramid nanofiber / polyimide composite aerogel. The aerogel exhibits excellent elasticity and ultra-low density (5.18g / cm 3 ), low thermal conductivity (0.0286W / (m·K)), high decomposition temperature (470℃), and maximum tolerance temperature of 200℃. [Materials Chemistry Frontiers, 2021, 5(2):804-816]. Zhang, Wang et al. reported a polyimide / silicon hybrid aerogel composite material with a small comprehensive shrinkage, moderate compression performance and excellent thermal stability, with a density of 0.152g / cm 3 , the comprehensive shrinkage rate is 3.52%, the compressive stress corresponding to 3% strain is 0.39MPa, the thermal conductivity is 0.0254W / (m·K), and the maximum tolerance temperature is 309℃. [ACS AppliedNano Materials.2023,6,9,7269-7279]. Fiber insulation materials are usually used on the leeward side of aircraft wings and fuselages at temperatures of 320-700℃. The high temperature resistance of the above-mentioned polyimide aerogel is still difficult to meet the needs of practical applications. Therefore, if the polyimide aerogel material can have better high temperature resistance while meeting the requirements of light weight, high strength and low thermal conductivity at room temperature and pressure, it will have incomparable advantages and broad application prospects. However, how to match the light weight, high strength, ultra-low thermal conductivity at room temperature and pressure and excellent high temperature resistance of polyimide aerogel has been a technical problem that has plagued the field of thermal insulation for many years. Summary of the invention
[0003] The purpose of the present invention is to solve the technical problem that the existing polyimide aerogel materials are difficult to match the performance requirements of high-performance organic thermal protection materials in the aerospace field, and to provide a high-temperature resistant polyimide aerogel composite material and its preparation method and application. The present invention is the first to create a one-way vacuum impregnation composite method for aerogel and fiber preforms, which maintains ultra-low thermal conductivity and low density at room temperature and pressure while increasing the tolerance temperature of polyimide aerogel and improving the mechanical strength, so that the prepared high-temperature resistant polyimide aerogel composite material meets the performance requirements of high-performance thermal protection materials in the current aerospace field.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: A method for preparing a high temperature resistant polyimide aerogel composite material comprises the following steps:
[0005] S1. Under ice bath stirring conditions, add diamine and dianhydride to an organic solvent respectively, and stir for 20 to 50 minutes to obtain a polyamic acid solution; the molar ratio of the diamine to the dianhydride is 1:1 to 1:1.4;
[0006] S2, adding a dehydrating agent to the polyamic acid solution, stirring, adding a metal oxide organic precursor or a non-metal oxide organic precursor, stirring until homogeneous, and then adding a catalyst and a cross-linking agent respectively, and continuously stirring until a polyimide sol is formed;
[0007] S3, compounding the polyimide sol with the prepared fiber preform by unidirectional vacuum impregnation, wherein the polyimide sol needs to completely immerse the prepared fiber preform; and then placing the fiber preform in an oven for heating and aging to form a fiber preform-reinforced polyimide initial gel;
[0008] S4, placing the fiber preform reinforced polyimide initial gel in a water bath set at a temperature of 45 to 90° C. and performing solvent replacement using an organic solvent, the solvent replacement is performed 3 to 8 times, and the solvent is replaced every 1 to 10 hours to obtain a fiber preform reinforced polyimide final gel;
[0009] S5. Drying the fiber preform reinforced polyimide final gel by CO2 supercritical fluid to obtain a fiber preform reinforced high temperature resistant polyimide aerogel composite material.
[0010] Preferably, the diamine in S1 is one or a mixture of p-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diamino-2,2'-dimethylbiphenyl, toluene diisocyanate, diphenylmethane diisocyanate; the dianhydride is one or a mixture of pyromellitic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, 3,3',4,4'-dibenzophenonetetracarboxylic anhydride, 4,4'-oxydiphthalic anhydride; the organic solvent is one or a mixture of dimethylacetamide, N,N-dimethylformamide, dimethyl phthalate, dimethyl sulfoxide, N-methylpyrrolidone.
[0011] Preferably, the dehydrating agent in S2 is a mixture of one or more of acetyl chloride, acetic anhydride, propionic anhydride, and thionyl chloride; the metal oxide organic precursor or non-metal oxide organic precursor is a mixture of one or more of ZrO2, triisopropoxy titanium chloride, chlorosilicate, Al2O3, diethylaluminum yne, B2O3, V2O5, CuO, copper ethylenediamine, copper acetate, and Fe2O3; the catalyst is a mixture of one or more of triethylamine, picoline, and pyridine; the cross-linking agent is a mixture of one or more of octaaminophenyl cage silsesquioxane, 1,3,5-tris(4-aminophenyl)benzene, triphenylmethane triisocyanate, 1,3,5-benzenetricarboxylic acid chloride, and 1,3,5-tris(4-aminophenoxy)benzene.
[0012] Preferably, the molar ratio of the dehydrating agent, the metal oxide organic precursor or the non-metal oxide organic precursor, the catalyst, the crosslinking agent and the diamine is 0.03-0.05:0.01-0.10:0.01-0.015:0.01-0.015:1.
[0013] Preferably, the fiber of the fiber preform in S3 is one or a combination of carbon fiber, quartz fiber, basalt fiber, glass fiber, zirconium dioxide fiber, polyimide fiber, mullite fiber, polyurethane fiber, aluminum silicate fiber, boron fiber, and the volume density of the fiber preform is 0.04-0.15 g / cm 3 .
[0014] Preferably, the temperature-raising aging in S3 is to raise the temperature to 20-50° C. and age for 18 hours.
[0015] More preferably, the organic solvent in S4 is methanol, ethanol, isopropanol or a mixture of several thereof.
[0016] Further preferably, the pressure of the CO2 supercritical fluid drying in S5 is 10-18 MPa, the temperature is 40-80°C, the drying time is 6-18 hours, and the pressure is released at a rate of 100-240 kPa / min after drying is completed.
[0017] The present invention also provides a high temperature resistant polyimide aerogel composite material prepared by the above preparation method.
[0018] The present invention also provides the use of the high temperature resistant polyimide aerogel composite material in the preparation of high performance thermal protection materials in the aerospace field.
[0019] The beneficial effects of the present invention are:
[0020] 1. In the second step of the preparation method of the high temperature resistant polyimide aerogel composite material of the present invention, a reinforcing phase such as a metal oxide organic precursor or a non-metal oxide organic precursor is innovatively added, and a cross-linking agent is added to introduce a cross-linking structure to enhance and modify the polyimide aerogel, thereby improving the stability of the molecular structure of the polyimide aerogel and the mutual support between the molecular chains, enhancing the network skeleton structure, and giving the polyimide aerogel excellent mechanical properties and thermal stability. In the third step, a unidirectional vacuum impregnation composite technology is used to perfectly composite the fiber preform with the aerogel, providing the aerogel with a stronger cross-linking degree and skeleton strength, greatly inhibiting the volume shrinkage of the aerogel, and further improving the high temperature resistance and mechanical properties of the polyimide aerogel composite material.
[0021] 2. The high temperature resistant polyimide aerogel composite material prepared by the method of the present invention can be used in an environment of up to 420°C, and the thermal decomposition temperature reaches 700°C. It has excellent high temperature resistance and strong thermal stability. The thermal conductivity at room temperature and pressure is 0.020-0.032 W / (m·K), and the density is 0.09-0.20 g / cm 3 The stress under 3% stress compression conditions is 0.3~0.8MPa, with low density and high strength, which better matches the current aerospace field's demand for lightweight, high-strength, high-performance organic thermal protection materials in the temperature range of 320~700℃. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention is a general flow chart of the method for preparing the high temperature resistant polyimide aerogel composite material. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0024] Embodiment 39
[0025] In the first step, p-phenylenediamine and pyromellitic anhydride were added to dimethylacetamide solvent in a ratio of 1:1.1 under ice bath stirring, and stirred for 45 minutes to obtain a polyamic acid solution.
[0026] In the second step, 0.05 parts (compared with the amount of diamine, the amount of diamine is recorded as 1 part, the same below) of acetic anhydride is added to 1 part of the polyamic acid solution prepared in the first step, and then 0.10 parts of ZrO2 are added. After stirring until homogeneous, 0.015 parts of methylpyridine and 0.015 parts of octaaminophenyl cage silsesquioxane are added respectively, and stirring is continued to form a polyimide sol.
[0027] In the third step, the polyimide sol prepared in the second step was mixed with 0.10 g / cm 3The basalt fiber preform is unidirectionally vacuum impregnated and compounded, and then aged in an oven at 30°C for 18 hours to form a fiber preform reinforced polyimide initial gel.
[0028] In the fourth step, the fiber preform reinforced polyimide initial gel prepared in the third step is placed in a 70° C. water bath for solvent replacement, and the organic solvent is used for replacement 4 times, and the solvent is replaced every 8 hours to obtain the fiber preform reinforced polyimide final gel.
[0029] The fifth step is to place the fiber preform reinforced polyimide final gel prepared in the fourth step into a CO2 supercritical drying device, heat it to 70°C, inject CO2 to 14MPa, dry it for 12h, and then slowly release the pressure at a rate of 170kPa / min to obtain a fiber preform reinforced high-temperature resistant polyimide aerogel composite material.
[0030] The density of the high temperature resistant polyimide aerogel composite material prepared in this embodiment is 0.194 g / cm 3 The thermal conductivity at room temperature and pressure is 0.0318W / (m·K), the compressive stress under 3% compressive strain conditions is 0.67MPa, and the maximum tolerable temperature is 420℃.
[0031] Embodiment 172
[0032] In the first step, 4,4'-diaminodiphenyl ether and 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added to N,N-dimethylformamide solvent in a ratio of 1:1.1 under ice bath stirring, and stirred for 45 minutes to obtain a polyamic acid solution.
[0033] In the second step, 0.05 parts (compared with the amount of diamine, the amount of diamine is recorded as 1 part, the same below) of acetic anhydride is added to 1 part of the polyamic acid solution prepared in the first step, and then 0.10 parts of triisopropoxytitanium chloride are added. After stirring until homogeneous, 0.015 parts of triethylamine and 0.015 parts of octaaminophenyl cage silsesquioxane are added respectively, and stirring is continued to form a polyimide sol.
[0034] In the third step, the polyimide sol prepared in the second step was mixed with 0.05 g / cm 3 The carbon fiber preform is subjected to single vacuum impregnation compounding and then aged in an oven at 30°C to form a fiber preform reinforced polyimide initial gel.
[0035] In the fourth step, the fiber preform reinforced polyimide initial gel prepared in the third step is placed in a 70° C. water bath for solvent replacement, and the organic solvent is used for replacement 4 times, and the solvent is replaced every 8 hours to obtain the fiber preform reinforced polyimide final gel.
[0036] The fifth step is to place the fiber preform reinforced polyimide final gel prepared in the fourth step into a CO2 supercritical drying device, heat it to 70°C, inject CO2 to 14MPa, dry it for 12h, and then slowly release the pressure at a rate of 170kPa / min to obtain a fiber preform reinforced high-temperature resistant polyimide aerogel composite material.
[0037] The density of the high temperature resistant polyimide aerogel composite material prepared in this embodiment is 0.181 g / cm 3 The thermal conductivity at room temperature and pressure is 0.0295W / (m·K), the compressive stress under 3% compressive strain conditions is 0.54MPa, and the maximum tolerable temperature is 382℃.
[0038] Embodiment 186
[0039] In the first step, 4,4'-diaminodiphenyl ether and 3,3',4,4'-biphenyltetracarboxylic dianhydride were added to dimethylacetamide solvent in a ratio of 1:1.1 under ice bath stirring, and stirred for 45 minutes to obtain a polyamic acid solution.
[0040] In the second step, 0.05 parts (compared with the amount of diamine, the amount of diamine is recorded as 1 part, the same below) of acetic anhydride is added to 1 part of the polyamic acid solution prepared in the first step, and then 0.10 parts of triisopropoxytitanium chloride are added. After stirring until homogeneous, 0.015 parts of methylpyridine and 0.015 parts of octaaminophenyl cage silsesquioxane are added respectively, and stirring is continued to form a polyimide sol.
[0041] In the third step, the polyimide sol prepared in the second step was mixed with 0.10 g / cm 3 The basalt fiber preform is subjected to single vacuum impregnation compounding and then aged in an oven at 30°C to form a fiber preform reinforced polyimide initial gel.
[0042] In the fourth step, the fiber preform reinforced polyimide initial gel prepared in the third step is placed in a 70° C. water bath for solvent replacement, and the organic solvent is used for replacement 4 times, and the solvent is replaced every 8 hours to obtain the fiber preform reinforced polyimide final gel.
[0043] The fifth step is to place the fiber preform reinforced polyimide final gel prepared in the fourth step into a CO2 supercritical drying device, heat it to 70°C, inject CO2 to 14MPa, dry it for 12h, and then slowly release the pressure at a rate of 170kPa / min to obtain a fiber preform reinforced high-temperature resistant polyimide aerogel composite material.
[0044] The density of the high temperature resistant polyimide aerogel composite material prepared in this embodiment is 0.190 g / cm 3The thermal conductivity at room temperature and pressure is 0.0308W / (m·K), the compressive stress under 3% compressive strain conditions is 0.79MPa, and the maximum tolerable temperature is 386℃.
[0045] Examples 1-38, 40-171, 173-185, 187-192
[0046] The preparation methods of Examples 1 to 38, 40 to 171, 173 to 185, and 187 to 192 are the same as those of Example 39, except that the process parameters used are as shown in Table 1, wherein the type of diamine, the type of dianhydride, the type of crosslinking agent, the type of metal oxide organic precursor or non-metal oxide organic precursor, the type of fiber preform, and the ratio of diamine to dianhydride are the main factors affecting the experimental data such as the density of the aerogel material, the thermal conductivity at room temperature and pressure, the mechanical strength performance, and the maximum tolerance temperature. The experimental process parameters not specified in the table have basically no effect on the above experimental data results of the aerogel material, and the aerogel of the present invention can be prepared as long as they are within the range described in the content of the invention. The specific parameters are shown in Table 1:
[0047] Table 1 Preparation process parameters of high temperature resistant polyimide aerogel composite materials
[0048]
[0049]
[0050]
[0051]
[0052]
[0053]
[0054]
[0055]
[0056]
[0057] From Examples 1 to 192, it can be seen that when octaaminophenyl cage silsesquioxane is selected as the cross-linking agent and basalt fiber is used as the fiber preform, and other parameters are fixed, the thermal conductivity of the aerogel at room temperature and pressure is low, and the maximum tolerable temperature is high. The thermal conductivity and maximum tolerable temperature of the polyimide aerogel at room temperature and pressure are mainly affected by the cross-linking agent and the fiber preform, the mechanical properties are mainly affected by the cross-linking agent, and the density is mainly affected by the type and proportion of the diamine and dianhydride. The present invention provides a lightweight, high-strength, high-temperature resistant polyimide aerogel composite material that can better match the current aerospace field's demand for high-performance organic thermal protection materials.
[0058] The specification and drawings of the present invention are considered to be illustrative rather than restrictive. On the basis of the present invention, those skilled in the art can make some substitutions and modifications to some of the technical features according to the disclosed technical content without creative labor, all of which are within the protection scope of the present invention.
Claims
1. A method for preparing a high temperature resistant polyimide aerogel composite material, characterized in that: The following steps are involved: S1. Under ice bath stirring conditions, taking diamine and dianhydride, respectively, adding them to an organic solvent, stirring for 20 to 50 minutes, to obtain a polyamic acid solution; the molar ratio of the diamine to the dianhydride is 1:1 to 1:1.4; S2, adding a dehydrating agent to the polyamic acid solution, stirring, adding a metal oxide organic precursor or a non-metal oxide organic precursor, stirring until homogeneous, and then adding a catalyst and a cross-linking agent respectively, and continuously stirring until a polyimide sol is formed; S3, compounding the polyimide sol with the prepared fiber preform by unidirectional vacuum impregnation, wherein the polyimide sol needs to completely immerse the prepared fiber preform; and then placing the fiber preform in an oven for heating and aging to form a fiber preform-reinforced polyimide initial gel; S4, placing the fiber preform reinforced polyimide initial gel in a water bath set at a temperature of 45 to 90° C. and performing solvent replacement using an organic solvent, the solvent replacement is performed 3 to 8 times, and the solvent is replaced every 1 to 10 hours to obtain a fiber preform reinforced polyimide final gel; S5. Drying the fiber preform reinforced polyimide final gel by CO2 supercritical fluid to obtain a fiber preform reinforced high temperature resistant polyimide aerogel composite material.
2. The preparation method according to claim 1, characterized in that: The diamine in S1 is one or a mixture of p-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diamino-2,2'-dimethylbiphenyl, toluene diisocyanate, and diphenylmethane diisocyanate; the dianhydride is one or a mixture of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-dibenzophenonetetracarboxylic dianhydride, and 4,4'-oxydiphthalic anhydride; and the organic solvent is one or a mixture of dimethylacetamide, N,N-dimethylformamide, dimethyl phthalate, dimethyl sulfoxide, and N-methylpyrrolidone.
3. The preparation method according to claim 1, characterized in that: The dehydrating agent in S2 is a mixture of one or more of acetyl chloride, acetic anhydride, propionic anhydride, and thionyl chloride; the metal oxide organic precursor or non-metal oxide organic precursor is a mixture of one or more of ZrO2, triisopropoxy titanium chloride, chlorosilicate, Al2O3, diethylaluminum yne, B2O3, V2O5, CuO, copper ethylenediamine, copper acetate, and Fe2O3; the catalyst is a mixture of one or more of triethylamine, methylpyridine, and pyridine; the cross-linking agent is a mixture of one or more of octaaminophenyl cage silsesquioxane, 1,3,5-tris(4-aminophenyl)benzene, triphenylmethane triisocyanate, 1,3,5-benzenetricarboxylic acid chloride, and 1,3,5-tris(4-aminophenoxy)benzene.
4. The preparation method according to claim 3, characterized in that: The molar ratio of the dehydrating agent, the metal oxide organic precursor or the non-metal oxide organic precursor, the catalyst, the crosslinking agent and the diamine is 0.03-0.05: 0.01-0.10: 0.01-0.015: 0.01-0.015:
1.
5. The preparation method according to claim 1, characterized in that: The fiber of the fiber preform in S3 is one or a combination of carbon fiber, quartz fiber, basalt fiber, glass fiber, zirconium dioxide fiber, polyimide fiber, mullite fiber, polyurethane fiber, aluminum silicate fiber, boron fiber, and the volume density of the fiber preform is 0.04-0.15 g / cm 3 .
6. The preparation method according to claim 1, characterized in that: The temperature-raising aging in S3 is to raise the temperature to 20-50° C. and age for 18 hours.
7. The preparation method according to claim 1, characterized in that: The organic solvent in S4 is one or a mixture of methanol, ethanol, isopropanol.
8. The preparation method according to claim 1, characterized in that: The CO2 supercritical fluid in S5 is dried at a pressure of 10-18 MPa, a temperature of 40-80°C, and a drying time of 6-18 hours. After drying, the pressure is released at a rate of 100-240 kPa / min.
9. The high temperature resistant polyimide aerogel composite material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the high temperature resistant polyimide aerogel composite material as claimed in claim 9 in the preparation of high performance thermal protection materials in the aerospace field.
Citation Information
Patent Citations
Light high-efficiency multilayer heat insulation material and preparation method thereof
CN110406135A
Flexible flame-retardant polyimide aerogel and preparation method thereof
CN110903511A
Polyimide aerogel composite material and preparation method thereof
CN111253742A
Multilayer structure composite high-temperature-resistant thermal protection material and preparation method thereof
CN111592369A
Controllable-structure thermal insulation material and preparation method thereof
CN112522852A
Cited By
Composite aerogel powder prepared by normal pressure method and preparation method thereof
CN119219972A
A method for preparing composite aerogel powder under atmospheric pressure and the preparation method thereof
CN119219972B
Preparation method of composite multifunctional PI aerogel
CN119978528A
A method for preparing a thermal shock resistant polyimide aerogel insulation material
CN120424406B
Aerogel-loaded thienyl conjugated polymer antibacterial agent as well as preparation method and application thereof
CN120460018A