Preparation method of regenerated rubber

By crushing, mixing and kneading multiple times, the plasticity and tear resistance of waste rubber are restored, and the problem of insufficient tear resistance in the preparation of existing recycled rubber is solved, and the efficient regeneration and environmentally friendly utilization of rubber is achieved.

CN118909306APending Publication Date: 2024-11-08SHENYANG RUBBER RES & DESIGN INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411314964.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the preparation of existing recycled rubber, the damage to the rubber molecular chain leads to a reduced tear resistance, limiting its scope of use.

Method used

Use a crusher to crush the waste rubber, mix pine tar, caprolactam and white carbon black, and then perform desulfurization reaction in a desulfurization tank, and kneading multiple times through a kneader, combining cooling and dehydration treatment to restore the plasticity and tear resistance of the rubber Cracking performance.

Benefits of technology

It improves the tear resistance of recycled rubber, expands its scope of use, and solves the problem of waste rubber polluting the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909306A_ABST
    Figure CN118909306A_ABST
Patent Text Reader

Abstract

The invention discloses a regenerated rubber preparation method which specifically comprises the following steps: S1, crushing cleaned and dried waste rubber into rubber powder with the particle size of 150-220 meshes by using a crusher, and weighing 100-150 parts by weight of the rubber powder, 15-20 parts by weight of pine tar, 5-8 parts by weight of caprolactam, 5-10 parts by weight of a tackifier and 3-5 parts by weight of white carbon black; s2, sequentially adding the rubber powder, the pine tar, the caprolactam, the tackifier and the white carbon black into a mixing mill, and mixing for 20-30 minutes at the mixing temperature of 100-150 DEG C; the invention belongs to the technical field of regenerated rubber preparation, and aims to solve the problem that in the prior art, the internal binding force of regenerated rubber is weakened, so that the tearing property is remarkably reduced. The regenerated rubber has the technical effects that the tackifier and the white carbon black are combined for use, so that the interaction force between the rubber can be increased, the tear resistance of the rubber is improved, and meanwhile, the plasticity of the regenerated rubber is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of regenerated rubber preparation, and in particular to a method for preparing regenerated rubber. Background Art

[0002] At present, in order to meet the ever-increasing material performance requirements, the rubber industry has improved the advantages of high strength, wear resistance and aging resistance of rubber through synthetic rubber during processing. However, this has caused the problem that the discarded rubber cannot be naturally degraded for a long time. The amount of waste rubber is huge and contains substances such as sulfur, causing serious black pollution;

[0003] The preparation of recycled rubber can replace natural rubber and synthetic rubber, alleviating the serious shortage of natural rubber and the economic cost waste of synthetic rubber processing; on the other hand, it realizes the recycling and reuse of waste rubber and solves the problem of waste rubber polluting the environment. The current process of recycled rubber preparation is to break some molecular chains and cross-linking points of vulcanized rubber under the combined action of plasticizers, oxygen, heat and mechanical shear, and then transform it into a re-vulcanizable rubber with plasticity and viscosity. However, the molecular chains of the recycled rubber are destroyed during the preparation process, resulting in the weakening of its internal bonding force, thereby significantly reducing the tear resistance of the recycled rubber, greatly limiting its scope of use and causing great inconvenience. Summary of the invention

[0004] To this end, the present invention provides a method for preparing recycled rubber to solve the above-mentioned problems in the prior art.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] According to a first aspect of the present invention, a method for preparing regenerated rubber comprises the following steps:

[0007] S1: Use a crusher to crush the washed and dried waste rubber into rubber powder with a particle size of 150-220 meshes, weigh 100-150 parts of rubber powder, 15-20 parts of pine tar, 5-8 parts of caprolactam, 5-10 parts of tackifier, and 3-5 parts of white carbon black;

[0008] S2: adding rubber powder, pine tar, caprolactam, tackifier and white carbon black into a mixer in sequence, mixing for 20-30 minutes at a mixing temperature of 100-150° C., and fully mixing to obtain a mixture;

[0009] S3: Add the mixture into a desulfurization tank with a stirrer and seal it, heat the desulfurization tank to 200℃-280℃, apply a pressure of 2.5-5MPa, control the desulfurization time to 5-8 hours and stir, and introduce clean air for 2-3 hours;

[0010] S4: The desulfurized rubber powder is discharged from the desulfurization tank, and immediately cooled and dehydrated, and then the dry rubber powder is added to the kneading machine, and the internal temperature of the kneading machine is controlled between 30-95°C, and the speed of the kneading machine is 60-80r / min for kneading, and the kneading time is 25-50 minutes;

[0011] S5: After kneading, cool for 2-3 hours, and repeat the kneading step in S4 for 5-8 times to obtain the final recycled rubber product.

[0012] Furthermore, the stirring speed of the stirrer in the desulfurization tank is 15-20r / min.

[0013] Furthermore, the specific steps of the cooling and dehydration treatment are as follows:

[0014] 1): Cool the rubber powder to 25-45℃ through cooling equipment, and the cooling time is controlled between 6-8 hours;

[0015] 2): Add the cooled rubber powder into a centrifugal dehydrator, control the speed of the centrifuge to 900r / min, dehydrate for 5-10 minutes, and obtain dry rubber powder.

[0016] Furthermore, the mass ratio of the tackifier to white carbon black is (2-3): (1-1.5).

[0017] The present invention has the following advantages:

[0018] 1. Pine tar is a softener, which softens the rubber powder to facilitate subsequent mixing and desulfurization treatment. Caprolactam is an activator, which mainly promotes the desulfurization reaction and improves the desulfurization efficiency. The combination of tackifier and white carbon black can increase the interaction force between rubbers, thereby improving the tear resistance of rubber.

[0019] 2. The rubber powder is desulfurized in a desulfurization tank, so that the rubber molecules in the rubber powder are degraded and cross-linked under the action of heat and pressure. At the same time, the network structure in the rubber powder is effectively destroyed and the plasticity is restored. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A flow chart of a method for preparing recycled rubber provided in some embodiments of the present invention. DETAILED DESCRIPTION

[0021] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] like Figure 1 As shown, a method for preparing recycled rubber in an embodiment of the first aspect of the present invention specifically comprises the following steps:

[0024] S1: Use a crusher to crush the washed and dried waste rubber into rubber powder with a particle size of 220 meshes, weigh 150 parts of rubber powder, 20 parts of pine tar, 8 parts of caprolactam, 10 parts of tackifier, and 4 parts of white carbon black by weight. Pine tar is a softener, which softens the rubber powder for subsequent mixing and desulfurization. Caprolactam is an activator, which mainly promotes the desulfurization reaction and improves the desulfurization efficiency. The combination of tackifier and white carbon black can increase the interaction force between rubbers, thereby improving the tear resistance of rubber. The mass ratio of tackifier to white carbon black is 2:1;

[0025] S2: adding rubber powder, pine tar, caprolactam, tackifier and white carbon black into a mixer in sequence, mixing for 20 minutes at a mixing temperature of 120° C., and fully mixing to obtain a mixture;

[0026] S3: Add the mixture into a desulfurization tank with an agitator and seal it. Heat the desulfurization tank to 260°C, apply a pressure of 5MPa, control the desulfurization time to 6 hours and stir, the stirring speed is 20r / min, and introduce clean air for 3 hours to improve the desulfurization reaction efficiency. The rubber molecules in the rubber powder are degraded and cross-linked and broken under the action of heating and pressure. At the same time, the network structure in the rubber powder is effectively destroyed and the plasticity is restored.

[0027] S4: The desulfurized rubber powder is discharged from the desulfurization tank, and immediately cooled and dehydrated, and then the dry rubber powder is added to the kneading machine, and the internal temperature of the kneading machine is controlled at 60°C, and the speed of the kneading machine is 80r / min for kneading, and the kneading time is 40 minutes;

[0028] S5: After kneading, cool for 2 hours, and repeat the kneading steps in S4 for 7 times, which can effectively improve the kneading effect of the rubber powder, thereby improving the plasticity and uniformity of the rubber, and helping to increase the tear resistance of the rubber, thereby obtaining the final recycled rubber product.

[0029] Cooling and dehydration treatment: cool the rubber powder to 45°C through cooling equipment, and the cooling time is controlled within 8 hours; add the cooled rubber powder to the centrifugal dehydrator, control the speed of the centrifuge to 900r / min, and dehydrate for 10 minutes to obtain dry rubber powder, so as to remove excess water and impurities in the rubber powder;

[0030] Example 2

[0031] A method for preparing recycled rubber, comprising the following steps:

[0032] S1: Use a crusher to crush the washed and dried waste rubber into rubber powder with a particle size of 150 meshes, and weigh 100 parts of rubber powder, 15 parts of pine tar, 5 parts of caprolactam, 5 parts of tackifier, and 5 parts of white carbon black;

[0033] S2: adding rubber powder, pine tar, caprolactam, tackifier and white carbon black into a mixer in sequence, mixing for 30 minutes at a mixing temperature of 150° C., and fully mixing to obtain a mixture;

[0034] S3: Add the mixture into a desulfurization tank with a stirrer and seal it, heat the desulfurization tank to 200°C, apply a pressure of 2.5MPa, control the desulfurization time to 8 hours and stir, and introduce clean air for 2 hours;

[0035] S4: The desulfurized rubber powder is discharged from the desulfurization tank, and immediately cooled and dehydrated, and then the dry rubber powder is added to a kneading machine, and the internal temperature of the kneading machine is controlled at 30°C, and the speed of the kneading machine is 60r / min for kneading, and the kneading time is 25 minutes;

[0036] S5: After kneading, cool for 3 hours, and repeat the kneading step in S4 8 times to obtain the final recycled rubber product;

[0037] Cooling and dehydration treatment: cool the rubber powder to 25°C through cooling equipment, and the cooling time is controlled within 6 hours; add the cooled rubber powder into a centrifugal dehydrator, control the speed of the centrifuge to 900r / min, and dehydrate for 8 minutes to obtain dry rubber powder, so as to remove excess water and impurities in the rubber powder.

[0038] It should be understood that these embodiments are only to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention.

Claims

1. A method for preparing recycled rubber, characterized in that: The specific steps include: S1: Use a crusher to crush the washed and dried waste rubber into rubber powder with a particle size of 150-220 meshes, weigh 100-150 parts of rubber powder, 15-20 parts of pine tar, 5-8 parts of caprolactam, 5-10 parts of tackifier, and 3-5 parts of white carbon black; S2: adding rubber powder, pine tar, caprolactam, tackifier and white carbon black into a mixer in sequence, mixing for 20-30 minutes at a mixing temperature of 100-150° C., and fully mixing to obtain a mixture; S3: Add the mixture into a desulfurization tank with a stirrer and seal it, heat the desulfurization tank to 200℃-280℃, apply a pressure of 2.5-5MPa, control the desulfurization time to 5-8 hours and stir, and introduce clean air for 2-3 hours; S4: The desulfurized rubber powder is discharged from the desulfurization tank, and immediately cooled and dehydrated, and then the dry rubber powder is added to the kneading machine, and the internal temperature of the kneading machine is controlled between 30-95°C, and the speed of the kneading machine is 60-80r / min for kneading, and the kneading time is 25-50 minutes; S5: After kneading, cool for 2-3 hours, and repeat the kneading step in S4 for 5-8 times to obtain the final recycled rubber product.

2. The method for preparing regenerated rubber according to claim 1, characterized in that: The stirring speed of the stirrer in the desulfurization tank is 15-20r / min.

3. The method for preparing regenerated rubber according to claim 1, characterized in that: The specific steps of the cooling and dehydration process are as follows: 1): Cool the rubber powder to 25-45℃ through cooling equipment, and the cooling time is controlled between 6-8 hours; 2): Add the cooled rubber powder into a centrifugal dehydrator, control the speed of the centrifuge to 900r / min, dehydrate for 5-10 minutes, and obtain dry rubber powder.

4. The method for preparing regenerated rubber according to claim 1, characterized in that: The mass ratio of the tackifier to white carbon black is (2-3): (1-1.5).