Micro-crosslinked high-density polyethylene film with enhanced yield strength and preparation method of micro-crosslinked high-density polyethylene film
By introducing peroxide crosslinking agents into high-density polyethylene to form a micro-crosslinked structure, the problem of low yield strength of high-density polyethylene film was solved, achieving an efficient film preparation process and improving the mechanical properties of the film.
Patent Information
- Application Number
- CN202410945347.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
AI Technical Summary
Existing high-density polyethylene films exhibit poor bubble stability and low yield strength during extrusion blown film production. Existing modification methods suffer from problems such as complex equipment, high energy consumption, or the generation of byproducts.
Peroxide crosslinking agent is blended with high-density polyethylene using a melt branching method, and a micro-crosslinked structure is formed by extruding through a twin-screw extruder. Then, a film is prepared by blown film under specific conditions.
It improves the yield strength of high-density polyethylene film, simplifies the process, saves costs, and avoids the degradation of polyethylene.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyethylene film preparation, and in particular to a micro-crosslinked high-density polyethylene film with enhanced yield strength and a preparation method thereof. Background Art
[0002] Polyethylene is easy to process, corrosion-resistant, and wear-resistant, and is one of the most widely used varieties of general synthetic plastics. High-density polyethylene is a type of polyethylene obtained by low-pressure catalytic polymerization. It has the characteristics of high crystallinity, high density, and high tensile strength. It can be used to prepare various films, containers, pipes, and other products through processes such as blow molding, injection molding, and extrusion. With the increasing demand for packaging materials in my country, the market demand for high-density polyethylene films continues to increase. However, the molecular chain of high-density polyethylene is basically linear, and there are almost no branches on the main chain. The degree of chain entanglement and melt strength are low when melted, resulting in poor bubble stability during extrusion blown film, and low yield strength of the prepared film. Micro-crosslinking can be achieved by introducing long branches into high-density polyethylene to transform its linear structure into a three-dimensional network structure. On the one hand, it improves the processing performance of high-density polyethylene, and on the other hand, it forms tie molecules between polyethylene lamellae, thereby increasing its yield strength.
[0003] At present, the industrial preparation methods of polyethylene long-chain branched structure include catalytic synthesis method and post-processing modification method. For example, patents US11267919B2 and USI1014997B2 use metallocene dual catalyst system to synthesize and produce long-chain branched high-density polyethylene for blown film applications. This method of catalytic synthesis of long-chain branched high-density polyethylene involves multi-step reactions, requires additional equipment, and has complex process conditions.
[0004] The main methods of post-processing modification include irradiating high-energy electron beams or rays in polyethylene with a crosslinking agent, or melt blending azo compounds or peroxides with polyethylene through an extruder to achieve long-chain branching. For example, in patent CN102030910A, high-energy electron beams or -rays are used to irradiate high-density polyethylene and mix it with matrix polyethylene and react to extrude it to prepare long-chain branched high-density polyethylene, thereby improving melt strength and mechanical properties. However, the high-energy irradiation method consumes a lot of energy, and the degree of crosslinking of polyethylene is difficult to control under high-energy irradiation, and it will degrade and produce by-products. In patent CN116239804A, 1,1-azo-radonyl cyclohexane is used to melt-react and extrude high-density polyethylene to prepare long-chain branched high-density polyethylene, thereby enhancing the melt strength of polyethylene. However, the decomposition temperature of azo compounds is relatively high, and blending and extruding with high-density polyethylene at high temperatures may degrade part of the polyethylene and produce by-products. Patent US11499023B2 uses 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and linear low-density polyethylene for melt reaction extrusion to enhance the melt strength of polyethylene and the yield strength of the film. The use of peroxides for long-chain branching modification is mainly used in the fields of linear low-density polyethylene films and high-density polyethylene pipes, and is rarely studied in the field of high-density polyethylene films. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a micro-crosslinked high-density polyethylene film with enhanced yield strength and a preparation method thereof. A peroxide-containing additive is blended and extruded with high-density polyethylene by a melt branching method. During the extrusion process, the polyethylene is modified with long chain branches and a micro-crosslinked structure is formed. Subsequently, the film is blown to obtain a high-density polyethylene film with higher yield strength.
[0006] To achieve the above objectives, the technical solution of the present invention is implemented through the following technical solutions:
[0007] A micro-crosslinked high-density polyethylene film with enhanced yield strength is composed of the following raw materials in parts by weight: 100 parts of high-density polyethylene and 0.01-0.20 parts of functional additives; the functional additives are a mixture of a base material and a peroxide crosslinking agent, wherein the peroxide crosslinking agent accounts for 1%-20% of the total weight of the functional additives, and the rest is the base material.
[0008] Preferably, the density of the high-density polyethylene is 0.950-0.958 g / cm 3The melt flow rate of the high-density polyethylene at 21.6 kg and 190° C. is 4-20 g / min, the ratio of the weight-average molecular weight to the number-average molecular weight is 20-35, there is no obvious double peak or multi-peak in the molecular weight distribution, and the loss factor in the dynamic rheological test at 190° C. and 0.1 rad / s is less than 1.3, and the high-density polyethylene is catalyzed by a titanium-based catalyst, wherein the magnesium content is less than 50 ppm.
[0009] Further preferably, the slightly cross-linked high-density polyethylene film is composed of the following raw materials in parts by weight: 100 parts of high-density polyethylene and 0.01-0.20 parts of functional additives.
[0010] Further preferably, the peroxide crosslinking agent in the functional additive accounts for 1%-20% of the total mass of the functional additive, and the rest is the base material.
[0011] Preferably, the peroxide crosslinking agent is any one of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, di-tert-butylperoxyisopropylbenzene, diisopropylbenzene peroxide, and 4,4-di(tert-butylperoxy)butyl valerate, or a mixture of several of them.
[0012] More preferably, the peroxide crosslinking agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.
[0013] Preferably, the base material is polyethylene or polypropylene, or a mixture of the two.
[0014] The method for preparing a micro-crosslinked high-density polyethylene film with enhanced yield strength comprises the following steps:
[0015] (1) premixing high-density polyethylene and functional additives to obtain a mixed material for later use;
[0016] (2) adding the mixed material into a twin-screw extruder for melt blending and extrusion granulation to obtain modified high-density polyethylene;
[0017] (3) blowing the high-density polyethylene film at a temperature of 195-210° C. and controlling the blowing speed to be 68-76 kg / h to obtain a slightly cross-linked high-density polyethylene film.
[0018] Preferably, the extrusion temperature in step (2) is 220-230° C., and the extrusion speed is 180-200 kg / h.
[0019] The present invention provides a micro-crosslinked high-density polyethylene film with enhanced yield strength and a preparation method thereof, which has the following advantages over the prior art:
[0020] The present invention adopts high-density polyethylene as a raw material and a peroxide-containing additive as a modifier. Long chain branches are introduced into the high-density polyethylene under twin-screw extrusion conditions to form micro-crosslinks. Subsequently, a film blowing machine is used to blow the modified high-density polyethylene under specific conditions to prepare a film. The prepared film has a high yield strength, and the entire process equipment is relatively simple and conventional. The entire processing process can save costs and prevent polyethylene degradation. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The density of the high-density polyethylene in the following examples and comparative examples is 0.954 g / cm 3 ; The melt flow rate (21.6kg, 190°C) is 15g / min, the ratio of weight-average molecular weight to number-average molecular weight is 25, there is no obvious bimodal or multimodal in the molecular weight distribution, the loss factor in the dynamic rheological test at 190°C and 0.1rad / s is less than 1.3, and the high-density polyethylene is catalyzed by a titanium-based catalyst, wherein the magnesium content is less than 50ppm; the composition of the functional additive is 90% polypropylene and 10% 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.
[0023] Embodiment 1:
[0024] 0.05 kg of functional additives were added to 100 kg of high-density polyethylene, and the mixture was placed in a twin-screw extruder and the extrusion temperature was adjusted to 225° C. and the extrusion rate was adjusted to 190 kg / h to obtain modified high-density polyethylene;
[0025] The modified high-density polyethylene is blown into film in the following two ways:
[0026] Method 1:
[0027] Film blowing is carried out under experimental film blowing conditions:
[0028] Adjust the extrusion temperature of the blown film at 210°C and control the die pressure at 168kgf / cm 2 , the die temperature was 210°C, the film blowing rate was controlled at 124 g / min, and a high-density polyethylene film was obtained;
[0029] Method 2:
[0030] Adopt industrial grade film blowing conditions for film blowing:
[0031] The extrusion temperature was controlled at 210°C and the film blowing rate was controlled at 74.3 kg / h to obtain a high-density polyethylene film.
[0032] The longitudinal tensile yield strength and transverse tensile yield strength of the high-density polyethylene films obtained by the two film blowing methods were tested respectively, and the specific results are shown in Table 1 below:
[0033] Table 1
[0034] Film blowing method Experimental film blowing conditions Industrial film blowing conditions Longitudinal tensile yield strength 29.0Mpa 29.2Mpa Transverse tensile yield strength 27.8Mpa 30.5Mpa
[0035] Comparative Example 1:
[0036] 0.1 kg of functional additives were added to 100 kg of high-density polyethylene, and the mixture was placed in a twin-screw extruder and the extrusion temperature was adjusted to 225° C. and the extrusion rate was adjusted to 190 kg / h to obtain modified high-density polyethylene;
[0037] The modified high-density polyethylene is blown into film in the following two ways:
[0038] Method 1:
[0039] Film blowing is carried out under experimental film blowing conditions:
[0040] Adjust the extrusion temperature of the blown film at 210°C and control the die pressure at 172kgf / cm 2 , the die temperature was 210°C, the film blowing rate was controlled at 131 g / min, and a high-density polyethylene film was obtained;
[0041] Method 2:
[0042] Adopt industrial grade film blowing conditions for film blowing:
[0043] The extrusion temperature was controlled at 210°C and the film blowing rate was controlled at 75.8 kg / h to obtain a high-density polyethylene film.
[0044] The longitudinal tensile yield strength and transverse tensile yield strength of the high-density polyethylene films obtained by the two film blowing methods were tested respectively, and the specific results are shown in Table 1 below:
[0045] Table 2
[0046] Film blowing method Experimental film blowing conditions Industrial film blowing conditions Longitudinal tensile yield strength 26.9Mpa 26.1Mpa Transverse tensile yield strength 27.2Mpa 26.2Mpa
[0047] Comparative Example 2:
[0048] The high-density polyethylene was placed in a twin-screw extruder and the extrusion temperature was adjusted to 225° C. and the extrusion rate was 190 kg / h to obtain a modified high-density polyethylene;
[0049] The modified high-density polyethylene is blown into film in the following two ways:
[0050] Method 1:
[0051] Film blowing is carried out under experimental film blowing conditions:
[0052] Adjust the extrusion temperature of the blown film at 210°C and control the die pressure at 168kgf / cm 2 , the die temperature was 210°C, the film blowing rate was controlled at 119 g / min, and a high-density polyethylene film was obtained;
[0053] Method 2:
[0054] Adopt industrial grade film blowing conditions for film blowing:
[0055] The extrusion temperature was controlled at 210°C and the film blowing rate was controlled at 68.3 kg / h to obtain a high-density polyethylene film.
[0056] The longitudinal tensile yield strength and transverse tensile yield strength of the high-density polyethylene films obtained by the two film blowing methods were tested respectively, and the specific results are shown in Table 3 below:
[0057] Table 3
[0058] Film blowing method Experimental film blowing conditions Industrial film blowing conditions Longitudinal tensile yield strength 27.3Mpa 29.6Mpa Transverse tensile yield strength 26.7Mpa 28.8Mpa
[0059] Comparative Example 3:
[0060] High-density polyethylene is directly blown into film in the following two ways:
[0061] Method 1:
[0062] Film blowing is carried out under experimental film blowing conditions:
[0063] Adjust the extrusion temperature of the blown film at 210°C and control the die pressure at 165kgf / cm 2 , the die temperature is 210°C, the film blowing rate is controlled at 100g / min, and a high-density polyethylene film is obtained;
[0064] Method 2:
[0065] Adopt industrial grade film blowing conditions for film blowing:
[0066] The extrusion temperature was controlled at 210°C and the film blowing rate was controlled at 57.6 kg / h to obtain a high-density polyethylene film.
[0067] The longitudinal tensile yield strength and transverse tensile yield strength of the high-density polyethylene films obtained by the two film blowing methods were tested respectively, and the specific results are shown in Table 4 below:
[0068] Table 4
[0069] Film blowing method Experimental film blowing conditions Industrial film blowing conditions Longitudinal tensile yield strength 24.3Mpa 27.9Mpa Transverse tensile yield strength 25.1Mpa 28.3Mpa
[0070] From the above tests, it can be seen that when functional additives are added to the mixed high-density polyethylene melt blend, controlling the industrial-grade film blowing conditions can effectively improve the longitudinal tensile and transverse tensile yield strength of the film.
[0071] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A micro-crosslinked high-density polyethylene film with enhanced yield strength, characterized in that: The micro-crosslinked high-density polyethylene film is composed of the following raw materials in parts by weight: 100 parts of high-density polyethylene and 0.01-0.20 parts of functional additives; the functional additives are a mixture of base material and peroxide crosslinking agent, wherein the peroxide crosslinking agent accounts for 1%-20% of the total weight of the functional additives, and the rest is the base material.
2. The slightly cross-linked high-density polyethylene film according to claim 1, characterized in that: The density of the high-density polyethylene is 0.950-0.958 g / cm 3 The melt flow rate of the high-density polyethylene at 21.6 kg and 190° C. is 4-20 g / min, the ratio of the weight-average molecular weight to the number-average molecular weight is 20-35, there is no obvious double peak or multi-peak in the molecular weight distribution, and the loss factor in the dynamic rheological test at 190° C. and 0.1 rad / s is less than 1.3, and the high-density polyethylene is catalyzed by a titanium-based catalyst, wherein the magnesium content is less than 50 ppm.
3. The slightly cross-linked high-density polyethylene film according to claim 1, characterized in that: The micro-crosslinked high-density polyethylene film is composed of the following raw materials in parts by weight: 100 parts of high-density polyethylene and 0.01-0.20 parts of functional additives.
4. The slightly cross-linked high-density polyethylene film according to claim 1, characterized in that: The peroxide crosslinking agent in the functional additive preferably accounts for 1%-20% of the total mass of the functional additive, and the rest is the base material.
5. The slightly cross-linked high-density polyethylene film according to claim 1, characterized in that: The peroxide crosslinking agent is any one of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, di-tert-butylperoxyisopropylbenzene, diisopropylbenzene peroxide, and 4,4-di(tert-butylperoxy)butyl valerate or a mixture of several of them.
6. The slightly cross-linked high-density polyethylene film according to claim 1, characterized in that: The base material is any one of polyethylene or polypropylene or a mixture of the two.
7. The slightly cross-linked high-density polyethylene film according to claim 1, characterized in that: The peroxide crosslinking agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.
8. A method for preparing a slightly cross-linked high-density polyethylene film according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) premixing high-density polyethylene and functional additives to obtain a mixed material for later use; (2) adding the mixed material into a twin-screw extruder for melt blending and extrusion granulation to obtain modified high-density polyethylene; (3) blowing the high-density polyethylene film at a temperature of 195-210° C. and controlling the blowing speed to be 57.6-74.3 kg / h to obtain a slightly cross-linked high-density polyethylene film.
9. The preparation method according to claim 4, characterized in that: The extrusion temperature in step (2) is 220-230° C., and the extrusion speed is 180-200 kg / h.
10. The preparation method according to claim 8, characterized in that: In the step (3), the modified high-density polyethylene is blended with other polyethylenes before film blowing, and the blending ratio of the modified high-density polyethylene is 5%-100%, so as to prepare a single-layer or multi-layer polyethylene film.
Citation Information
Patent Citations
Method for preparing long chain branched polyethylene
CN102030910A
Long-chain branched high-density polyethylene and preparation method thereof
CN116239804A
Dual catalyst system for producing polyethylene with long chain branching for blow molding applications
US11267919B2
Peroxide treated metallocene-based polyolefins with improved melt strength
US11499023B2