High-temperature-resistant high-toughness epoxy resin and preparation method thereof

By adding a specific proportion of toughening agent and curing agent to the epoxy resin and controlling the reaction conditions, high-temperature and high-toughness epoxy resin is prepared, which solves the problem that epoxy resins in the prior art are difficult to achieve high temperature resistance and high toughness at the same time. , achieves stable performance and toughness improvement at higher temperatures, and is suitable for aviation composite materials manufacturing.

CN118909403APending Publication Date: 2024-11-08CHENGDU AIRCRAFT INDUSTRY GROUP
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410970548.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing aviation epoxy resins are difficult to achieve high temperature resistance and high toughness at the same time, which limits their application scope in the aviation field.

Method used

By mixing epoxy resin, toughener, aromatic diamine curing agent and temperature-rheology-regulating components in a specific proportion, and controlling the reaction temperature and stirring time, the dry glass transition temperature after curing was prepared at 210°C after curing. ~220°C, high-temperature and high-toughness epoxy resin with a shear strength retention rate of more than 50% between layers under saturated hygroscopic conditions.

Benefits of technology

The high-temperature stability and toughness of epoxy resin have been improved, and the impact strength reaches 45KJ/m2~52KJ/m2, meeting the manufacturing needs of aviation composite parts with higher temperature requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909403A_ABST
    Figure CN118909403A_ABST
Patent Text Reader

Abstract

The invention discloses high-temperature-resistant high-toughness epoxy resin and a preparation method thereof, relates to the technical field of composite materials, and particularly aims to solve the technical problem that the application range of the epoxy resin in the aviation field is limited due to the defect that high temperature resistance and high toughness are difficult to realize at the same time in the conventional aviation epoxy resin. The high-temperature-resistant and high-toughness epoxy resin is prepared by mixing 60 to 110 parts of an epoxy resin component, 5 to 35 parts of a toughening agent component, 10 to 30 parts of an aromatic diamine curing agent component and 0 to 15 parts of a temperature-resistant and rheological adjusting component, the dry glass transition temperature of the cured high-temperature-resistant and high-toughness epoxy resin is 210-220 DEG C; the glass transition temperature under the saturated moisture absorption condition is 157-165 DEG C, the interlaminar shear strength retention rate is greater than 50% under the condition of 130 DEG C after saturated moisture absorption, and the impact strength is 45KJ / m < 2 >-52KJ / m < 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite materials, and in particular to a high-temperature resistant and high-toughness epoxy resin and a preparation method thereof. Background Art

[0002] At present, the main composite materials used in the aviation field are fiber-reinforced resin-based composite materials based on thermosetting bismaleimide and epoxy resin. In comparison, epoxy resin-based composite materials have better toughness and stable part molding processability, so they are easier to meet the damage tolerance design requirements of aircraft. However, its disadvantage is that its temperature resistance is not as good as that of bismaleimide composite materials, so it cannot fully meet the manufacturing needs of composite parts for high-speed aviation equipment, and its application is limited.

[0003] In response to this problem, foreign countries have successively developed a number of aviation-grade high-temperature resistant epoxy resins, with long-term use temperatures of up to 130°C or even higher. Composite materials based on such resins have been successfully used in supersonic manned aircraft such as the F-22. However, due to the limitations of technical level, domestic aviation-grade epoxy resins are mainly resins with long-term use temperatures ≤80°C, and are therefore mainly used in low-speed UAVs and civil aviation equipment. Although the development of high-temperature resistant epoxy resins has emerged in an endless stream in China in recent years, and the composite materials prepared therefrom have gradually been used in a small number of aviation equipment, the problem of reduced resin toughness and other mechanical properties caused by the improvement of temperature resistance has not been well solved, resulting in the scope of high-temperature epoxy being still limited.

[0004] In order to solve the above problems, it is urgent to develop an epoxy resin matrix with excellent high temperature resistance and toughness to meet the requirements for the use of aviation composite materials. Summary of the invention

[0005] The present application provides a high-temperature resistant and high-toughness epoxy resin and a preparation method thereof, aiming to solve the technical problem that the existing aviation epoxy resin is difficult to achieve high temperature resistance and high toughness at the same time, which limits its application scope in the aviation field.

[0006] To solve the above technical problems, the embodiment of the present application provides: a high temperature resistant and high toughness epoxy resin, which is prepared by mixing 60 to 110 parts of epoxy resin components, 5 to 35 parts of toughening agent components, 10 to 30 parts of aromatic diamine curing agent components and 0 to 15 parts of temperature resistance-rheology adjustment components; the high temperature resistant and high toughness epoxy resin has a dry glass transition temperature of 210°C to 220°C after curing; the glass transition temperature under saturated moisture absorption conditions is 157°C to 165°C, the interlaminar shear strength retention rate is greater than 50% when placed at 130°C after saturated moisture absorption, and the impact strength is 45KJ / m 2 ~52KJ / m 2 .

[0007] As some optional embodiments of the present application, the epoxy resin component is a mixed prepolymer of bisphenol A epoxy resin and phenolic epoxy resin.

[0008] As some optional embodiments of the present application, the toughening agent component is a mixture of thermoplastic phenolphthalein type polyaryletherketone resin, thermoplastic phenolphthalein type polyimide resin, thermoplastic phenolphthalein type polyethersulfone resin and inorganic nano-silicon particles.

[0009] As some optional embodiments of the present application, the curing agent component is at least one aromatic amine curing agent.

[0010] As some optional embodiments of the present application, the temperature resistance-rheology regulating component is a mixed prepolymer of a multifunctional epoxy resin and a liquid cyanate ester resin.

[0011] In order to solve the above technical problems, the present application also proposes: a method for preparing the high temperature resistant and high toughness epoxy resin as described above, comprising the following steps:

[0012] The epoxy resin component, the first preset amount of toughening agent component, the temperature resistance-rheology adjustment component, the second preset amount of toughening agent component and the aromatic diamine curing agent component are sequentially added into the reaction kettle for reaction. After the reaction is completed, the epoxy resin composition is obtained after cooling to room temperature.

[0013] As some optional embodiments of the present application, the epoxy resin component, the preset first amount of toughening agent component, the temperature resistance-rheology adjustment component, the preset second amount of toughening agent component and the aromatic diamine curing agent component are added to the reactor at different temperature conditions.

[0014] As some optional embodiments of the present application, the temperatures of the epoxy resin component and the preset first amount of toughening agent component when added to the reactor>the temperature of the temperature-resistant-rheology adjustment component when added to the reactor>the temperature of the preset second amount of toughening agent component when added to the reactor≥the temperature of the aromatic diamine curing agent component when added to the reactor.

[0015] As some optional embodiments of the present application, the temperature of the epoxy resin component and the preset first amount of toughening agent component when added to the reaction kettle is 130° C. to 150° C.;

[0016] The temperature of the temperature-resistant and rheology-adjusting component when added to the reactor is 85°C to 95°C;

[0017] The temperature of the preset second amount of toughening agent component when added into the reactor is 70°C to 80°C;

[0018] The temperature of the aromatic diamine curing agent component when added into the reaction kettle is 70°C.

[0019] As some optional embodiments of the present application, the step of sequentially adding an epoxy resin component, a preset first amount of a toughening agent component, a temperature resistance-rheology adjustment component, a preset second amount of a toughening agent component and an aromatic diamine curing agent component into a reaction kettle for reaction, and after the reaction is completed, cooling to room temperature to obtain an epoxy resin composition comprises:

[0020] Add the epoxy resin component and the first amount of the toughening agent component to a reaction kettle at 130° C. to 150° C., mix, and stir for 30 min to 60 min; wherein the epoxy resin component and the toughening agent component are used in a ratio of 100:5 to 22;

[0021] Lower the temperature of the reactor to 85°C to 95°C, add the temperature-resistant and rheology-adjusting components, and stir for 20min to 30min until uniform;

[0022] After the temperature of the reactor is lowered to 70°C to 80°C, a toughening agent component is added to the mixture, and stirred for 10-20 minutes until uniform; wherein the ratio of the mixture to the toughening agent is 100:3-15;

[0023] The temperature of the reactor was maintained at 70°C, and the aromatic diamine curing agent component was added and stirred for 10-20 minutes;

[0024] After cooling to room temperature, an epoxy resin composition was obtained.

[0025] Compared with the prior art, the high temperature resistant and high toughness epoxy resin described in the present application is prepared by mixing 60 to 110 parts of epoxy resin components, 5 to 35 parts of toughening agent components, 10 to 30 parts of aromatic diamine curing agent components and 0 to 15 parts of temperature resistance-rheology adjustment components. The epoxy resin prepared by mixing the above components has an impact strength of 45KJ / m after curing. 2 ~52KJ / m 2 , which is better than the impact strength data reported in the literature. At the same time, the dry glass transition temperature of the resin is between 210℃ and 220℃, and the glass transition temperature of the prepared composite material under saturated moisture absorption conditions is between 157℃ and 165℃. After saturated moisture absorption, the interlaminar shear strength test is carried out at 130℃. The test results show that the interlaminar shear strength of the resin in this state is greater than 50% compared with the data obtained in the dry state at room temperature, and it can be used for a long time at 130℃. The high-temperature and high-toughness epoxy resin of this application can be used for the manufacture of aviation composite parts with higher temperature requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific embodiments of the present application or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the prior art description. In all drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0027] Figure 1 This is a schematic diagram of the preparation process of the high temperature resistant and high toughness epoxy resin described in the embodiments of the present application;

[0028] Figure 2 This is the test graph of the glass transition temperature of the epoxy resin described in Experimental Example 1 of this application;

[0029] Figure 3 This is a test diagram of the glass transition temperature of the epoxy resin described in Experimental Example 3 of this application;

[0030] Figure 4 This is a diagram of the laminate forming process parameters described in Experimental Example 2 of this application.

[0031] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0033] It should be noted that all directional indications in the embodiments of the present application (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0034] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present application, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes. Taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0035] At present, the main composite materials used in the aviation field are fiber-reinforced resin-based composite materials based on thermosetting bismaleimide and epoxy resin. In comparison, epoxy resin-based composite materials have better toughness (easier to meet the damage tolerance design requirements of aircraft) and stable part molding processability. However, its disadvantage is that its temperature resistance is not as good as that of bismaleimide composite materials, so it cannot fully meet the manufacturing needs of composite parts for high-speed aviation equipment, and its application is limited.

[0036] In response to this problem, foreign countries have successively developed a number of aviation-grade high-temperature resistant epoxy resins, with long-term use temperatures of up to 130°C or even higher. Composite materials based on such resins have been successfully used in supersonic manned aircraft such as the F-22. However, due to the limitations of technical level, domestic aviation-grade epoxy resins are mainly resins with long-term use temperatures ≤80°C, and are therefore mainly used in low-speed UAVs and civil aviation equipment. Although the development of high-temperature resistant epoxy resins has emerged in an endless stream in China in recent years, and the composite materials prepared therefrom have gradually been used in a small number of aviation equipment, the problem of reduced resin toughness and other mechanical properties caused by the improvement of temperature resistance has not been well solved, resulting in the scope of high-temperature epoxy being still limited.

[0037] In order to solve the above problems, it is necessary to develop an epoxy resin matrix with excellent high temperature resistance and toughness to meet the requirements for the use of aviation composite materials.

[0038] That is, the existing aviation epoxy resins have the disadvantage of being difficult to achieve high temperature resistance and high toughness at the same time, which limits their application scope in the aviation field. Therefore, the purpose of this application is to provide a high-temperature and high-toughness epoxy resin formulation for the preparation of epoxy prepregs and resin-based composite materials. It is required to be able to meet long-term use at 130°C (required indicators: dry glass transition temperature ≥210°C after resin curing; glass transition temperature of composite materials under saturated moisture absorption conditions ≥155°C, and the interlaminar shear strength retention rate of composite materials placed at 130°C after saturated moisture absorption is not less than 50%), while having excellent toughness (required indicators: impact strength ≥40KJ / ㎡) and other properties.

[0039] Specifically, the high temperature resistant and high toughness epoxy resin described in the present application is prepared by mixing 60 to 110 parts of epoxy resin components, 5 to 35 parts of toughening agent components, 10 to 30 parts of aromatic diamine curing agent components and 0 to 15 parts of temperature resistance-rheology adjustment components; the high temperature resistant and high toughness epoxy resin has a dry glass transition temperature of 210°C to 220°C after curing; the glass transition temperature under saturated moisture absorption conditions is 157°C to 165°C, the interlaminar shear strength retention rate is greater than 50% when placed at 130°C after saturated moisture absorption, and the impact strength is 45KJ / m 2 ~52KJ / m 2 .

[0040] It should be noted that the epoxy resin component is a mixed prepolymer of bisphenol A epoxy resin and phenolic epoxy resin; the toughening agent component is a mixture of thermoplastic phenolphthalein type polyaryletherketone resin, thermoplastic phenolphthalein type polyimide resin, thermoplastic phenolphthalein type polyethersulfone resin and inorganic nano-silicon particles; the curing agent component is at least one aromatic amine curing agent; the temperature resistance-rheology adjustment component is a mixed prepolymer of multifunctional epoxy resin and liquid cyanate resin.

[0041] It can be seen that the present application adopts a method in which a prepolymer of conventional E epoxy resin and phenolic epoxy resin is used as the main body of epoxy resin to ensure that the resin has good usability and processability. At the same time, a prepolymer of multifunctional epoxy resin and cyanate resin is innovatively used as a temperature and rheology regulator to ensure the temperature resistance and process window of the resin, and a thermoplastic phenolphthalein type resin with good film-forming and toughening effects is used as a toughening agent. By adjusting the ratio and preparation process parameters of the main resin, toughening agent, modifier and curing agent, an epoxy resin with both high temperature resistance and good toughness is designed. The results of the present invention can be used in the manufacture of high-performance aviation resin-based composite parts.

[0042] That is: by using a mixed prepolymer of bisphenol A epoxy resin and phenolic epoxy resin, the cured resin has both the excellent chemical resistance of bisphenol A epoxy resin and the high temperature stability of phenolic epoxy resin, thereby improving the comprehensive performance of the resin. By adding a mixture of thermoplastic phenolphthalein polyaryletherketone resin, polyimide resin, polyethersulfone resin and inorganic nano-silicon particles as a toughening agent, the toughness and impact resistance of the resin can be effectively improved, thereby reducing the risk of breakage during use. By selecting at least one aromatic amine curing agent, this curing agent has good curing effect and chemical stability, which helps to ensure that the resin can achieve the expected performance indicators after curing. By using a mixed prepolymer of multifunctional epoxy resin and liquid cyanate resin as a temperature-resistant-rheological adjustment component, the rheological properties and thermal stability of the resin can be adjusted, so that the cured resin still maintains good performance in a high temperature environment.

[0043] In summary, the selection and proportion of these specific components make the resulting epoxy resin have high temperature stability, excellent toughness, moisture resistance and good curing effect, making it widely applicable and reliable in various engineering applications.

[0044] The preparation process of the high temperature resistant and high toughness epoxy resin described in this application is described in detail below:

[0045] A method for preparing the high temperature resistant and high toughness epoxy resin as described above comprises the following steps:

[0046] The epoxy resin component, the first preset amount of toughening agent component, the temperature resistance-rheology adjustment component, the second preset amount of toughening agent component and the aromatic diamine curing agent component are sequentially added into the reaction kettle for reaction. After the reaction is completed, the epoxy resin composition is obtained after cooling to room temperature.

[0047] It should be noted that the epoxy resin component, the preset first amount of toughening agent component, the temperature resistance-rheology adjustment component, the preset second amount of toughening agent component and the aromatic diamine curing agent component are added to the reactor at different temperature conditions. More specifically, the temperature of the epoxy resin component and the preset first amount of toughening agent component when added to the reactor> the temperature of the temperature resistance-rheology adjustment component when added to the reactor> the temperature of the preset second amount of toughening agent component when added to the reactor≥the temperature of the aromatic diamine curing agent component when added to the reactor.

[0048] It should be noted that in the preparation process of epoxy resin, the temperature control when adding different components into the reactor is to optimize the reaction kinetics and ensure the quality and performance of the final product. With regard to the temperature sequence described above, there are several key considerations for setting it:

[0049] The epoxy resin component and the first amount of toughening agent component are added at a higher temperature: These two components are usually basic reaction components and need to be added at a higher temperature to promote sufficient mixing and dissolution. The higher temperature helps the fluidity of the epoxy resin and the uniform distribution of the toughening agent, thereby ensuring that the reaction proceeds evenly and avoiding local aggregation or unevenness of the components.

[0050] Temperature-resistant rheology-adjusting components are added at a slightly lower temperature: These components are added at a lower temperature to control the rheological properties (such as viscosity) and reaction rate of the resin. Too high a temperature may cause these components to react too quickly or become unstable, thus affecting the performance of the final product. Properly lowering the addition temperature can maintain the activity of the components and allow them to be evenly distributed in the resin.

[0051] The second amount of toughening agent component and aromatic diamine curing agent component is added at a lower temperature: the curing agent, especially the aromatic diamine curing agent, has high reactivity and needs to be added at a lower temperature to avoid premature reaction or uncontrollable side reactions. The lower addition temperature helps to maintain the activity of the curing agent, so that it can effectively promote the cross-linking reaction during the subsequent heating and curing process. At the same time, the second addition of the toughening agent may be to further improve its properties, such as impact toughness, when the resin is basically formed. This also needs to be done at a lower temperature to avoid affecting the already formed network structure.

[0052] Through this graded temperature addition strategy, the reaction process can be more effectively controlled to ensure that each component can be added under the most suitable conditions, maximize its effectiveness, and ultimately obtain an epoxy resin product with excellent performance.

[0053] In some specific embodiments, the temperature of the epoxy resin component and the preset first amount of toughening agent component when added to the reactor is 130°C to 150°C; the temperature of the temperature-resistant-rheology adjustment component when added to the reactor is 85°C to 95°C; the temperature of the preset second amount of toughening agent component when added to the reactor is 70°C to 80°C; the temperature of the aromatic diamine curing agent component when added to the reactor is 70°C.

[0054] In combination with the above technical features, the preparation process will be further described below. Figure 1 As shown, the step of sequentially adding an epoxy resin component, a preset first amount of a toughening agent component, a temperature resistance-rheology adjustment component, a preset second amount of a toughening agent component and an aromatic diamine curing agent component into a reaction kettle for reaction, and after the reaction is completed, cooling to room temperature to obtain an epoxy resin composition comprises:

[0055] Step S10, adding the epoxy resin component and the preset first amount of toughening agent component into a reaction kettle at 130° C. to 150° C., mixing, and stirring for 30 min to 60 min; wherein the usage ratio of the epoxy resin component to the toughening agent component is 100:5 to 22;

[0056] Step S20, lowering the temperature of the reactor to 85°C to 95°C, adding a temperature-resistant and rheology-adjusting component, and stirring for 20min to 30min until uniform;

[0057] Step S30, after lowering the temperature of the reactor to 70°C to 80°C, adding a toughening agent component to the mixture, and stirring for 10-20 minutes until uniform; wherein the ratio of the mixture to the toughening agent is 100:3-15;

[0058] Step S40, maintaining the temperature of the reactor at 70° C., adding an aromatic diamine curing agent component, and stirring for 10-20 minutes;

[0059] Step S50, cooling to room temperature to obtain an epoxy resin composition.

[0060] It can be seen that the preparation method described in this application has the following advantages:

[0061] Good temperature control: Different temperature stages are used in the scheme, and each stage has a corresponding temperature range and duration. This temperature control ensures that different components react at the appropriate temperature, promoting the uniformity and efficiency of the reaction.

[0062] The reaction process is carried out step by step: The scheme divides the reaction process into multiple stages, and different components are added gradually. This step-by-step approach helps control the reaction rate and temperature, reduces the impact of uncontrollable factors, and improves the stability and consistency of the product.

[0063] Sufficient stirring time: Sufficient stirring time is provided at each stage to ensure sufficient mixing and dissolution of the components. Sufficient stirring time can promote uniform reaction and prevent component agglomeration or local unevenness.

[0064] Stable product quality: By precisely controlling the temperature and reaction process, the quality stability of the product can be improved. This stability is not only reflected in the consistency of product performance, but also reduces the difference between batches, improves production efficiency and product reliability.

[0065] The operation is relatively simple: Although it includes multiple steps, the operation of each step is relatively simple and clear, easy to implement and control. This helps to reduce the operational risk and error rate in the production process and improve production efficiency and product quality.

[0066] In summary, the technical solution described in the present application effectively optimizes the preparation process of epoxy resin through reasonable temperature control, gradual reaction, sufficient stirring and other measures, improves the quality and stability of the product, and also improves production efficiency and ease of operation.

[0067] In order to facilitate those skilled in the art to further understand the technical solution described in the present application, the technical solution described in the present application will be described below in conjunction with specific embodiments:

[0068] Example 1

[0069] Weigh 78 parts of bisphenol A epoxy resin E54 and 20 parts of phenolic epoxy resin o-cresol epoxy, heat to 130°C and stir until the prepolymer is completely uniform. Then add 7 parts of phenolphthalein polyaryletherketone toughening agent, then heat to 145°C, stir for 1h, cool to 95°C, then add 10 parts of m-aminophenol triglycidyl epoxy resin and bisphenol A cyanate prepolymer (prepolymerization temperature: 140°C), stir for 10min. Then cool to 75°C, add 3 parts of phenolphthalein polyaryletherketone toughening agent, stir evenly, and then add 28 parts of aromatic diamine curing agent. After being uniform, bag and obtain the resin product.

[0070] Experimental Example 1

[0071] Resin performance test:

[0072] The prepared epoxy resin was cured at 180°C for 3h to prepare a casting, and the cured product was tested. The test results are as follows: Figure 2 As shown, the dry glass transition temperature of the resin is 216.01℃ (DMA method, 5℃ / min), the impact strength is 51.1KJ / ㎡ (pendulum impact method, GB / T 2567), and other properties are shown in Table 1:

[0073] Table 1 Other properties of high temperature epoxy resin

[0074]

[0075] Experimental Example 2

[0076] Composite material performance testing

[0077] T700 grade domestic unidirectional carbon fiber (specification 12K) is selected as the fiber raw material and combined with resin to prepare prepreg. The designed resin content is 34±2%, the fiber surface density is 133±3g / ㎡, and the single layer thickness after curing is 0.125±0.01mm. The prepreg is prepared by a two-step hot melt method (hot melt coating + hot melt dipping) molding process.

[0078] like Figure 4 As shown, the composite mechanical laminate is prepared according to the following process:

[0079] 1) After leak detection, apply vacuum pressure ≤-0.90bar.

[0080] 2) Set the pressure to 6.5 Bar for 10 minutes. Set the temperature to 135°C at a rate of 2°C / min. When the leading thermocouple reaches 130°C, start timing and keep the temperature constant for 60 minutes.

[0081] 3) After the constant temperature is completed, set the temperature to 181°C at a rate of 2°C / min. When the lagging thermocouple reaches 177°C, start timing and keep the constant temperature for 182 minutes.

[0082] 4) After the constant temperature is completed, set the temperature to ≤60℃ at a rate of 1.5℃ / min. When the lagging thermocouple is cooled to ≤65℃, release the pressure to 0Bar.

[0083] 5) When the temperature of the lagging thermocouple drops to ≤60℃, release the vacuum and take the tank out.

[0084] The prepared composite material was subjected to saturated moisture absorption (boiling in boiling water for 72 hours), and its wet glass transition degree was measured by DMA method (5℃ / min) to be 160.5℃. Subsequently, the interlaminar shear specimen was processed and tested according to ASTM 2344, and its interlaminar shear strength under 130℃ wet conditions was measured to be 49.7MPa. Another non-moisture-absorbed test piece was selected and tested according to the same method, and its value was measured to be 98.0MPa, and the strength retention rate was 50.7%. Other properties, such as the longitudinal tensile modulus retention rate under 130℃ wet conditions was 96.6%, and the flexural modulus retention rate was 97.3%.

[0085] Example 2

[0086] Weigh 65 parts of E54 epoxy resin and 35 parts of o-cresol epoxy resin, heat to 130°C and stir until the prepolymer is completely uniform. Then cool it to 50-60°C, add 8 parts of phenolphthalein polyaryletherketone toughening agent, then heat to 145°C, stir for 1h, cool to 95°C, then add 12 parts of m-aminophenol triglycidyl epoxy resin and bisphenol A cyanate prepolymer (prepolymerization temperature: 140°C), stir for 10min. Then cool to 75°C, add 3 parts of thermoplastic phenolphthalein polyethersulfone toughening agent, stir evenly, and then add 30 parts of aromatic diamine curing agent. After being uniform, bag it to obtain the resin product.

[0087] Experimental Example 3

[0088] Resin performance test:

[0089] The prepared epoxy resin was also cured at 180°C for 3 hours to prepare a casting, and the cured product was tested. The test results are as follows: Figure 3As shown, the dry glass transition temperature of the resin is 213.99℃ (DMA method, 5℃ / min), and the impact strength is 44.4KJ / ㎡ (pendulum impact method, GB / T 2567). Other properties of the resin are shown in Table 2:

[0090] Table 2 Other properties of high temperature epoxy resin

[0091]

[0092] Experimental Example 4

[0093] Composite material performance test:

[0094] The same T700-grade domestic unidirectional carbon fiber (specification 12K) as in Experimental Example 2 was selected as the fiber raw material and combined with resin to prepare the prepreg. The designed resin content was 35±2%, the fiber surface density was 133±3g / ㎡, and the single layer thickness after curing was 0.125±0.01mm. The prepreg was also prepared by a two-step hot melt method (hot melt coating + hot melt dipping) molding process.

[0095] The preparation process of the composite material mechanical laminate is exactly the same as that of Experimental Example 2.

[0096] The prepared composite material was subjected to saturated moisture absorption (boiling in boiling water for 72 hours), and its wet glass transition degree was measured by DMA method (5℃ / min) to be 158.6℃. Subsequently, the interlaminar shear specimen was processed and tested according to ASTM 2344, and its interlaminar shear strength under 130℃ wet conditions was measured to be 47.5MPa. Another non-moisture-absorbed test piece was selected and tested according to the same method, and its value was measured to be 93.4MPa, and the strength retention rate was 50.9%. Other properties, such as the longitudinal tensile modulus retention rate measured under 130℃ wet conditions was 93.9%, and the flexural modulus retention rate was 97.7%.

[0097] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A high temperature resistant and high toughness epoxy resin, characterized in that: The high temperature resistant and high toughness epoxy resin is prepared by mixing 60 to 110 parts of epoxy resin components, 5 to 35 parts of toughening agent components, 10 to 30 parts of aromatic diamine curing agent components and 0 to 15 parts of temperature resistance-rheology regulating components; the high temperature resistant and high toughness epoxy resin has a dry glass transition temperature of 210 to 220° C. after curing; a glass transition temperature of 157 to 165° C. under saturated moisture absorption conditions, an interlaminar shear strength retention rate of more than 50% at 130° C. after saturated moisture absorption, and an impact strength of 45 KJ / m 2 ~52KJ / m 2 .

2. The high temperature resistant and high toughness epoxy resin according to claim 1, characterized in that: The epoxy resin component is a mixed prepolymer of bisphenol A epoxy resin and phenolic epoxy resin.

3. The high temperature resistant and high toughness epoxy resin according to claim 1, characterized in that: The toughening agent component is a mixture of thermoplastic phenolphthalein type polyaryletherketone resin, thermoplastic phenolphthalein type polyimide resin, thermoplastic phenolphthalein type polyethersulfone resin and inorganic nano silicon particles.

4. The high temperature resistant and high toughness epoxy resin according to claim 1, characterized in that: The curing agent component is at least one aromatic amine curing agent.

5. The high temperature resistant and high toughness epoxy resin according to claim 1, characterized in that: The temperature resistance and rheology regulating component is a mixed prepolymer of multifunctional epoxy resin and liquid cyanate resin.

6. A method for preparing a high temperature resistant and high toughness epoxy resin as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: The epoxy resin component, the first preset amount of toughening agent component, the temperature resistance-rheology adjustment component, the second preset amount of toughening agent component and the aromatic diamine curing agent component are sequentially added into the reaction kettle for reaction. After the reaction is completed, the epoxy resin composition is obtained after cooling to room temperature.

7. The method for preparing the high temperature resistant and high toughness epoxy resin according to claim 6, characterized in that: The epoxy resin component, the preset first amount of toughening agent component, the temperature resistance-rheology adjustment component, the preset second amount of toughening agent component and the aromatic diamine curing agent component are added to the reaction kettle at different temperature conditions.

8. The method for preparing the high temperature resistant and high toughness epoxy resin according to claim 7, characterized in that: The temperature of the epoxy resin component and the preset first amount of toughening agent component when added to the reactor>the temperature of the heat-resistant-rheology regulating component when added to the reactor>the temperature of the preset second amount of toughening agent component when added to the reactor≥the temperature of the aromatic diamine curing agent component when added to the reactor.

9. The method for preparing the high temperature resistant and high toughness epoxy resin according to claim 7, characterized in that: The temperature of the epoxy resin component and the preset first amount of toughening agent component when added into the reaction kettle is 130° C. to 150° C.; The temperature of the temperature-resistant and rheology-adjusting component when added to the reactor is 85°C to 95°C; The temperature of the preset second amount of toughening agent component when added into the reactor is 70°C to 80°C; The temperature of the aromatic diamine curing agent component when added into the reaction kettle is 70°C.

10. The method for preparing the high temperature resistant and high toughness epoxy resin according to claim 6, characterized in that: The step of sequentially adding an epoxy resin component, a preset first amount of a toughening agent component, a temperature resistance-rheology adjustment component, a preset second amount of a toughening agent component and an aromatic diamine curing agent component into a reaction kettle for reaction, and after the reaction is completed, cooling to room temperature to obtain an epoxy resin composition comprises: Add the epoxy resin component and the first amount of the toughening agent component to a reaction kettle at 130° C. to 150° C., mix, and stir for 30 min to 60 min; wherein the epoxy resin component and the toughening agent component are used in a ratio of 100:5 to 22; Lower the temperature of the reactor to 85°C to 95°C, add the temperature-resistant and rheology-adjusting components, and stir for 20min to 30min until uniform; After the temperature of the reactor is lowered to 70°C to 80°C, a toughening agent component is added to the mixture, and stirred for 10-20 minutes until uniform; wherein the ratio of the mixture to the toughening agent is 100:3-15; The temperature of the reactor was maintained at 70°C, and the aromatic diamine curing agent component was added and stirred for 10-20 minutes; After cooling to room temperature, an epoxy resin composition was obtained.

Citation Information

Cited By

  • Heat-resistant epoxy resin and preparation method thereof

    CN120137357A

  • A heat-resistant epoxy resin and a method for preparing the same

    CN120137357B

  • Aviation thermosetting composite material with low forming temperature and preparation method thereof

    CN120682601A