Single-component curable gel and preparation method thereof

By preparing a single-component curable gel and controlling the specific ratio and melting point of phase change-platinum catalyst particles, the extrusion and storage problems of two-component gels were solved, achieving stable storage and efficient curing at room temperature.

CN118909445APending Publication Date: 2024-11-08SHANGHAI DUYU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410973688.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing two-component gels have insufficient extrudability during construction, and the gel is difficult to store when hydrogen-containing silicone oil is present, which cannot effectively improve extrudability.

Method used

A single-component curable gel preparation method is adopted. First, phase change-platinum catalyst particles are prepared and mixed with silicone oil, filler, additives and alkynol inhibitors. By controlling the ratio of phase change material and platinum catalyst and the hot melting point, it is ensured that the gel does not solidify at room temperature and has good storage properties. When in use, heating is used to liquefy the phase change material and carry out secondary mixing to promote cross-linking and curing.

Benefits of technology

It improves the extrudability and storage properties of the gel, ensuring stable storage at room temperature. It can be effectively cured by heating during use, thus improving the crosslinking efficiency during the extrusion process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004953939460000061
    Figure BDA0004953939460000061
Patent Text Reader

Abstract

The invention relates to the technical field of phase change materials, in particular to the field of IPC C08L83, and more particularly relates to single-component curable gel and a preparation method thereof. The silicone oil phase change material is prepared from the following components in parts by weight: 5 to 20 parts of silicone oil, 80 to 95 parts of filler, 0.05 to 0.5 part of additive, 0.03 to 0.5 part of alkynol inhibitor, 0.1 to 0.7 part of phase change material and 0.02 to 0.5 part of platinum catalyst. Firstly, phase change-platinum catalyst particles are prepared and then mixed with a gel system, and the single-component gel with stable performance can be prepared. The weight ratio of the phase change material to the platinum catalyst is (8-9): (1-2), the hot melting point of the phase change material is limited to be 40-90 DEG C, the viscosity at the hot melting point is not greater than 2000 cps, and the extrudability of the gel can be further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of phase change materials, in particular to the field of IPC C08L83, and more specifically to a single-component curable gel and a preparation method thereof. Background Art

[0002] Phase change materials are materials that can absorb heat (cold) from the environment during the phase change process (the process of phase change materials changing from solid to liquid or from liquid to solid is called phase change process) and release heat (cold) to the environment when needed, thereby achieving the purpose of controlling the temperature of the surrounding environment. Phase change materials have the advantages of high heat storage density, small temperature and volume changes, low corrosiveness and stable chemical properties. They can effectively improve the utilization rate of non-renewable energy. They are green, energy-saving and environmentally friendly materials that play a vital role in the development of new energy and thermal energy storage. The reason is that phase change materials mainly include aliphatic hydrocarbons, fatty acids, alcohols and olefins, which make them less prone to phase separation, overcooling and low corrosiveness. Two-component gel needs to be mixed in a mixing head during construction, and its extrudability will drop significantly during the mixing process. To deal with this problem, the thixotropy is usually adjusted, or the original gel viscosity is changed to increase the extrudability. However, this method is greatly affected by the performance of the filler and the raw material itself, which is far from the extrudability of the gel itself. In view of the above scenarios, it is necessary to improve the difficulty of gel storage when hydrogenated silicone oil coexists and the problem of insufficient extrudability of filled gel during mixing.

[0003] CN117070068A discloses an organic silicon foam for phase change material and a preparation method thereof, which is prepared by the following raw materials in parts by weight: component A: 100 parts of base material, 20-30 parts of diluent, 5-30 parts of foaming agent, and 0.5-1.5 parts of platinum catalyst; component B: 100 parts of base material, 15-30 parts of functional filler, 10-15 parts of diluent, 20-30 parts of hydrogen-containing silicone oil, and 0.3-0.4 parts of inhibitor. The organic silicon foam for phase change material prepared by adopting the above formula has the advantages of low density, high porosity, good absorbency and good compressibility, but the phase change material only plays a packaging role and is still a two-component system. Summary of the invention

[0004] The first aspect of the present invention provides a one-component curable gel, which comprises, by weight, 5-20 parts of silicone oil, 80-95 parts of filler, 0.05-0.5 parts of additives, 0.03-0.5 parts of acetylene alcohol inhibitors, 0.1-0.7 parts of phase change materials, and 0.02-0.5 parts of platinum catalysts.

[0005] Preferably, the components include, by weight: 10-20 parts of silicone oil, 80-95 parts of filler, 0.05-0.3 parts of additives, 0.03-0.3 parts of acetylene alcohol inhibitors, 0.1-0.2 parts of phase change materials, and 0.02-0.1 parts of platinum catalysts.

[0006] Preferably, the weight ratio of the acetylene alcohol inhibitor to the platinum catalyst is (0.1-0.2):(0.02-0.08).

[0007] The silicone oil includes hydrogen-containing silicone oil and vinyl silicone oil, and the weight ratio of the hydrogen-containing silicone oil to the vinyl silicone oil is 1:(0.25-4).

[0008] The hydrogen-containing silicone oil includes at least one of single-terminal silicone oil, double-terminal silicone oil, side-chain silicone oil, and single-terminal blocked silicone oil.

[0009] The viscosity of the silicone oil at 25° C. is 20-500 cps.

[0010] The vinyl silicone oil contains vinyl groups at both ends and side chains.

[0011] The alkynol inhibitor includes at least one of 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol, and 2-phenyl-3-butyn-2-ol.

[0012] The filler particle size is at least one of the following: 0.2-1 micron, 2-5 microns, 5-20 microns, 20-70 microns, 70-120 microns.

[0013] The phase change material includes at least one of hot-melt tackifying resin, polyester resin and paraffin.

[0014] The phase change material has a thermal melting point of 40-90° C., and a viscosity at the thermal melting point of no more than 2000 cps.

[0015] The filler includes at least one of aluminum oxide, boron nitride, aluminum nitride, diamond, zinc oxide, aluminum, and aluminum hydroxide.

[0016] Preferably, the filler includes at least one of aluminum oxide, boron nitride and aluminum nitride.

[0017] The auxiliary agent includes at least one of γ-aminopropyl triethoxysilane, γ-glycidyloxypropyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, decyl trimethoxysilane, dodecyl trimethoxysilane and hexadecyl trimethoxysilane.

[0018] The second aspect of the present invention provides a method for preparing a one-component curable gel, comprising the following steps:

[0019] S1, melting the phase change material, adding a platinum catalyst to make it uniformly mixed, and sequentially cooling-crushing-blocking-ball milling to obtain phase change-platinum catalyst particles;

[0020] S2, vacuum stirring the silicone oil, filler, additive, acetylene alcohol inhibitor and phase change-platinum catalyst particles to obtain.

[0021] Preferably, the weight ratio of the phase change material to the platinum catalyst is (8-9):(1-2).

[0022] The phase change-platinum catalyst particles have a D50 particle size of 0.1-20 microns, a sphericity of ≥90%, and a specific surface area of ​​20-50 m 2 / g.

[0023] The applicant has found that by first preparing phase change-platinum catalyst particles and then mixing them with a gel system, a single-component gel with stable performance can be prepared. Further research has found that the weight ratio of the phase change material and the platinum catalyst is (8-9): (1-2), and the thermal melting point of the phase change material is limited to 40-90°C. The viscosity at the thermal melting point is not more than 2000cps, which can further improve the extrusion of the gel. In this way, vinyl and hydrogen-containing silicone oil can be placed in the same component to form a gel for room temperature storage. In actual application, the phase change material-platinum catalyst is uniformly dispersed in the gel in a solid state. When used, heating is selected to liquefy the phase change material-platinum catalyst and perform secondary mixing during the extrusion process. The different specific surface areas of the phase change material before and after the phase change material are used to increase the contact surface between the catalyst and the gel to promote the cross-linking and curing of the gel. Compared with the prior art, the single-component curable gel stored at room temperature changes the acetylene alcohol-catalyst ratio in the product through phase change, so that the two-component gel can be mixed into the same component. When the thermal melting point is not reached, the catalyst is coated by the phase change, so that the single-component gel does not produce cross-linking under the action of the acetylene alcohol inhibitor; when used, the temperature rises to the thermal melting point and the coated catalyst is mixed twice during the extrusion process, so that the effect of the acetylene alcohol inhibitor decreases and cross-linking begins.

[0024] Beneficial effects:

[0025] 1. Phase change-platinum catalyst particles are first prepared and then mixed with the gel system to prepare a single-component gel with stable performance.

[0026] 2. The weight ratio of the phase change material and the platinum catalyst is (8-9): (1-2), and the thermal melting point of the phase change material is limited to 40-90°C, and the viscosity at the thermal melting point is not more than 2000cps, which can further improve the extrudability of the gel.

[0027] 3. The gel prepared in the present application does not solidify at room temperature under a specific acetylene alcohol-platinum catalyst mass ratio, and its storage performance is effectively improved.

[0028] 4. The gel prepared in the present application can be extruded when the thermal melting point of the phase change-platinum catalyst particles exceeds the thermal melting point and can be solidified at room temperature. DETAILED DESCRIPTION

[0029] Example 1

[0030] A single-component curable gel comprises, by weight, 10 parts of silicone oil, 89 parts of filler, 0.2 parts of auxiliary agent, 0.2 parts of acetylene alcohol inhibitor, 0.54 parts of phase change material and 0.06 parts of platinum catalyst.

[0031] The silicone oil is hydrogen-containing silicone oil (Runhe RH-H6) and vinyl silicone oil (Runhe RH-Vi1311), and the weight ratio of the hydrogen-containing silicone oil to the vinyl silicone oil is 1:(0.25-4).

[0032] The filler is aluminum, boron nitride, and aluminum nitride, and the weight ratio of aluminum, boron nitride, and aluminum nitride is 90:10:10. The D10 particle size of the filler is 1 micron, the D50 particle size is 10 microns, the D90 particle size is 40 microns, and the D100 particle size is 70 microns.

[0033] The auxiliary agent is Evonik's silane coupling agent, hexadecyltrimethoxysilane, model: 9116.

[0034] The inhibitor is 1-ethynyl-1-cyclohexanol (Aladdin Reagent Co., Ltd.).

[0035] The phase change material is phase change paraffin (Kunlun-58, phase change thermal melting point temperature is 50-55°C).

[0036] The platinum catalyst was purchased from Shanghai Platinum World, model: pt3000.

[0037] A method for preparing a one-component curable gel comprises the following steps:

[0038] S1, melt the phase change material, add platinum catalyst, heat and mix (temperature 80°C), stop stirring after 30 minutes, cool until the surface of the mixture is crusted, quickly take out the material for physical crushing, and grind it with a Lansbury grinder. The obtained powder is then ball milled, and the phase change-platinum catalyst mixture is obtained by reciprocating plug-ball milling to obtain phase change-platinum catalyst particles (1200 mesh);

[0039] S2, vacuum stirring the silicone oil, filler, additive, acetylene alcohol inhibitor and phase change-platinum catalyst particles to obtain.

[0040] Example 2

[0041] A single-component curable gel comprises, by weight, 10 parts of silicone oil, 89 parts of filler, 0.2 parts of auxiliary agent, 0.3 parts of acetylene alcohol inhibitor, 0.45 parts of phase change material and 0.05 parts of platinum catalyst.

[0042] The silicone oil is hydrogen-containing silicone oil (Runhe RH-H6) and vinyl silicone oil (Runhe RH-Vi1311), and the weight ratio of the hydrogen-containing silicone oil to the vinyl silicone oil is 1:(0.25-4).

[0043] The filler is aluminum, boron nitride, and aluminum nitride, and the weight ratio of aluminum, boron nitride, and aluminum nitride is 90:10:10. The D10 particle size of the filler is 1 micron, the D50 particle size is 10 microns, the D90 particle size is 40 microns, and the D100 particle size is 70 microns.

[0044] The auxiliary agent is Evonik's silane coupling agent, hexadecyltrimethoxysilane, model: 9116.

[0045] The inhibitor is 1-ethynyl-1-cyclohexanol (Aladdin Reagent Co., Ltd.).

[0046] The phase change material is phase change paraffin (Kunlun-58, phase change thermal melting point temperature is 50-55°C).

[0047] The platinum catalyst was purchased from Shanghai Platinum World, model: pt3000.

[0048] A method for preparing a one-component curable gel comprises the following steps:

[0049] S1, melt the phase change material, add platinum catalyst, heat and stir (temperature 80°C), stop stirring after 30 minutes, cool until the surface of the mixture forms a crust, quickly take out the material for physical crushing, and grind it with a Lansbury grinder. The obtained powder is then ball milled, and the phase change-platinum catalyst mixture is obtained by repeated plug-ball milling to obtain phase change-platinum catalyst particles;

[0050] S2, vacuum stirring the silicone oil, filler, additive, acetylene alcohol inhibitor and phase change-platinum catalyst particles to obtain.

[0051] Example 3

[0052] A single-component curable gel comprises, by weight, 10 parts of silicone oil, 89 parts of filler, 0.2 parts of auxiliary agent, 0.6 parts of acetylene alcohol inhibitor, 0.18 parts of phase change material and 0.02 parts of platinum catalyst.

[0053] The silicone oil is hydrogen-containing silicone oil (Runhe RH-H6) and vinyl silicone oil (Runhe RH-Vi1311), and the weight ratio of the hydrogen-containing silicone oil to the vinyl silicone oil is 1:(0.25-4).

[0054] The filler is aluminum, boron nitride, and aluminum nitride, and the weight ratio of aluminum, boron nitride, and aluminum nitride is 90:10:10. The D10 particle size of the filler is 1 micron, the D50 particle size is 10 microns, the D90 particle size is 40 microns, and the D100 particle size is 70 microns.

[0055] The auxiliary agent is Evonik's silane coupling agent, hexadecyltrimethoxysilane, model: 9116.

[0056] The inhibitor is 1-ethynyl-1-cyclohexanol (Aladdin Reagent Co., Ltd.).

[0057] The phase change material is phase change paraffin (Kunlun-58, phase change thermal melting point temperature is 50-55°C).

[0058] The platinum catalyst was purchased from Shanghai Platinum World, model: pt3000.

[0059] A method for preparing a one-component curable gel comprises the following steps:

[0060] S1, melt the phase change material, add platinum catalyst, heat and stir (temperature 80°C), stop stirring after 30 minutes, cool until the surface of the mixture forms a crust, quickly take out the material for physical crushing, and grind it with a Lansbury grinder. The obtained powder is then ball milled, and the phase change-platinum catalyst mixture is obtained by repeated plug-ball milling to obtain phase change-platinum catalyst particles;

[0061] S2, vacuum stirring the silicone oil, filler, additive, acetylene alcohol inhibitor and phase change-platinum catalyst particles to obtain.

[0062] Example 4

[0063] A single-component curable gel comprises, by weight, 10 parts of silicone oil, 89 parts of filler, 0.2 parts of auxiliary agent, 0.1 parts of acetylene alcohol inhibitor, 0.81 parts of phase change material and 0.19 parts of platinum catalyst.

[0064] The silicone oil is hydrogen-containing silicone oil (Runhe RH-H6) and vinyl silicone oil (Runhe RH-Vi1311), and the weight ratio of the hydrogen-containing silicone oil to the vinyl silicone oil is 1:(0.25-4).

[0065] The filler is aluminum, boron nitride, and aluminum nitride, and the weight ratio of aluminum, boron nitride, and aluminum nitride is 90:10:10. The D10 particle size of the filler is 1 micron, the D50 particle size is 10 microns, the D90 particle size is 40 microns, and the D100 particle size is 70 microns.

[0066] The auxiliary agent is Evonik's silane coupling agent, hexadecyltrimethoxysilane, model: 9116.

[0067] The inhibitor is 1-ethynyl-1-cyclohexanol (Aladdin Reagent Co., Ltd.).

[0068] The phase change material is phase change paraffin (Kunlun-58, phase change thermal melting point temperature is 50-55°C).

[0069] The platinum catalyst was purchased from Shanghai Platinum World, model: pt3000.

[0070] A method for preparing a one-component curable gel comprises the following steps:

[0071] S1, melt the phase change material, add platinum catalyst, heat and stir (temperature 80°C), stop stirring after 30 minutes, cool until the surface of the mixture forms a crust, quickly take out the material for physical crushing, and grind it with a Lansbury grinder. The obtained powder is then ball milled, and the phase change-platinum catalyst mixture is obtained by repeated plug-ball milling to obtain phase change-platinum catalyst particles;

[0072] S2, vacuum stirring the silicone oil, filler, additive, acetylene alcohol inhibitor and phase change-platinum catalyst particles to obtain.

[0073] Performance Testing Methods

[0074] The examples 1 to 4 were packaged in 30cc tubes, and the gel was squeezed onto the release film using a glue gun, and the following tests were performed: 25°C surface dry test, 35°C surface dry test, and 45°C surface dry test; refer to GB / T 13477.5 finger touch test standard. The test data are listed in Table 1.

[0075] The gels of Examples 1 to 4 were packaged in 30cc tubes, and the gels were placed in a 60°C oven and baked for 30 minutes for the following tests: 25°C surface dry test, 35°C surface dry test, and 45°C surface dry test; refer to GB / T 13477.5 finger touch test standard. The test data are listed in Table 2.

[0076] The surface is qualified if it dries for 30-90 minutes, otherwise it is unqualified.

[0077] The gel of Example 3 was packaged in 50CC tubes (the packaging tubes were 50CC two-component tubes produced by Shenzhen PuShen Company); 6 tubes were required; 3 of them were without mixing heads, and 3 were equipped with mixing heads. The extrusion properties of the above 2 groups of gels were tested with reference to the GB / T13477.3 test standard, and the extrusion properties test was performed for 1 minute at a pressure of 90Psi using a Lambawan-866 dispensing machine.

[0078] Performance test data

[0079] Table 1

[0080]

[0081]

[0082] Table 2

[0083] 25℃ Surface dry / min 35℃ Surface dry / min 45℃ Surface dry / min Example 1 Failed (250min) Failed (180min) Pass (90min) Example 2 Failed (180min) Failed (135min) Pass (80min) Example 3 Failed (140min) Failed (95min) Pass(35min) Example 4 Pass (90min) Pass (60min) Failed (10min)

[0084] Table 3

[0085] Without mixing head g / min With mixing head g / min Test 1 95 15 Test 2 91 14.5 Test 3 96 14.8 average value 94 14.8

[0086] It can be seen from Table 1-2 that under the condition of a specific mass ratio of acetylene alcohol-platinum catalyst in the example gel, it does not solidify at room temperature and its storage performance is effectively improved; when the gel exceeds the thermal melting point of the phase change-platinum catalyst mixture and is extruded, it can be solidified at room temperature.

[0087] As shown in Table 3, after comparing the extrudability of the gel in the example before and after passing through the mixing tube, the extrudability is effectively improved, and the extrudability of the highly filled gel is significantly improved.

Claims

1. A one-component curable gel, characterized in that: The components include, by weight: 5-20 parts of silicone oil, 80-95 parts of filler, 0.05-0.5 parts of additive, 0.03-0.5 parts of acetylene alcohol inhibitor, 0.1-0.7 parts of phase change material, and 0.02-0.5 parts of platinum catalyst.

2. The one-component curable gel according to claim 1, characterized in that The silicone oil includes hydrogen-containing silicone oil and vinyl silicone oil, and the weight ratio of the hydrogen-containing silicone oil to the vinyl silicone oil is 1:(0.25-4).

3. The one-component curable gel according to claim 2, characterized in that The hydrogen-containing silicone oil includes at least one of single-end silicone oil, double-end silicone oil, side-chain silicone oil, and single-end blocked silicone oil.

4. The one-component curable gel according to claim 3, characterized in that The viscosity of the silicone oil at 25° C. is 20-500 cps.

5. The one-component curable gel according to claim 4, characterized in that The vinyl silicone oil contains vinyl groups at both ends and side chains.

6. The one-component curable gel according to claim 5, characterized in that The alkynol inhibitor includes at least one of 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol, and 2-phenyl-3-butyn-2-ol.

7. The one-component curable gel according to claim 6, characterized in that The filler particle size is at least one of the following: 0.2-1 micron, 2-5 microns, 5-20 microns, 20-70 microns, 70-120 microns.

8. A method for preparing the one-component curable gel according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, melting the phase change material, adding a platinum catalyst to make it uniformly mixed, and sequentially cooling-crushing-blocking-ball milling to obtain phase change-platinum catalyst particles; S2, vacuum stirring the silicone oil, filler, additive, acetylene alcohol inhibitor and phase change-platinum catalyst particles to obtain.

9. The method for preparing a one-component curable gel according to claim 8, characterized in that: The weight ratio of the phase change material to the platinum catalyst is (8-9):(1-2).

10. The method for preparing a one-component curable gel according to claim 8, characterized in that: The phase change-platinum catalyst particles have a D50 particle size of 0.1-20 microns, a sphericity of ≥90%, and a specific surface area of ​​20-50 m 2 / g.