High-temperature-resistant odorless asphalt composition and preparation method thereof

By using zinc ricinoleate fat, porous dispersant and activated zinc powder in asphalt, the problems of damaged high-temperature performance and harmful gas emissions are solved, and efficient deodorization and performance improvements are achieved. It is suitable for multiple Types of asphalt.

CN118909455APending Publication Date: 2024-11-08XIAMEN SUNLIT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411150601.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Most of the existing asphalt deodorizing components are liquid materials, which leads to damage to the high-temperature performance of asphalt and cannot effectively reduce the emission of harmful gases during high temperatures, affecting construction personnel and the environment.

Method used

Using zinc ricinoleate fat, porous dispersant and activated zinc powder as the main components, a high-temperature odor-resistant asphalt composition is prepared through specific mixing and heating treatment, which significantly improves the high-temperature performance of asphalt. and deodorization effect.

Benefits of technology

It significantly improves the high-temperature resistance and odor removal effect of asphalt, reduces the emission of harmful gases, maintains good high-temperature performance and reduces the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909455A_ABST
    Figure CN118909455A_ABST
Patent Text Reader

Abstract

The invention provides a high-temperature-resistant odorless asphalt composition and a preparation method thereof, and belongs to the technical field of road engineering materials.The asphalt composition is prepared from, by weight, 90-99 parts of asphalt and 1-10 parts of an odorless agent, and the odorless agent is prepared from zinc ricinoleate, a porous dispersing agent and activated zinc powder. The preparation method comprises the following steps: mixing and stirring a porous dispersant and activated zinc powder for 30-60 minutes to obtain a first mixture; heating the first mixture to 80-100 DEG C, adding zinc diricinoleate into the first mixture, stirring for 6-12 hours, and standing at room temperature for 24-48 hours to obtain an odor removing agent; the method comprises the following steps: weighing 90-99 parts of asphalt and 1-10 parts of an odorless agent, and mixing the asphalt and the odorless agent to obtain the asphalt composition. The asphalt composition can inhibit smoke generated in the high-temperature process, meanwhile, gas reaction components are dispersed in the porous material, the reaction efficiency is greatly improved, and the high-temperature performance of asphalt can be effectively improved by taking the inorganic porous dispersion material as filler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road engineering materials, and in particular relates to a high temperature resistant and odorless asphalt composition and a preparation method thereof. Background Art

[0002] Asphalt and asphalt mixtures produce many harmful gases during production, transportation and construction. Among them, sulfides, such as hydrogen sulfide, sulfur dioxide and mercaptans, also have pungent odors, which greatly affect the physical and mental health of construction workers and the progress of construction. At the same time, the exhaust gas affects the surrounding residents. Therefore, it is very necessary to conduct early treatment of the exhaust gas generated by asphalt during high temperature, reduce its emission, and reduce the impact on the environment and people.

[0003] Nowadays, asphalt deodorizers are mainly odor masking agents, most of which use added fragrance ingredients to mask the pungent odor of asphalt and asphalt mixtures produced under high temperature conditions, which actually cannot reduce the emission of harmful gases. Some deodorizers achieve the purpose of reducing emissions through chemical reactions, but most of their components are liquid materials, which inevitably damages the high-temperature performance of asphalt and reduces the high-temperature performance of asphalt pavement.

[0004] In view of this, the present application proposes a high-temperature resistant and odorless asphalt composition and a preparation method thereof, which can suppress the smoke generated during the high-temperature process of asphalt, effectively improve the high-temperature performance of asphalt, and the product maintains good results for a long time. Summary of the invention

[0005] In order to solve the problem that the existing asphalt deodorizer components are mostly liquid materials, which inevitably leads to damage to the high-temperature performance of asphalt, etc., the purpose of the present invention is to propose a high-temperature resistant odor-free asphalt composition and a preparation method thereof to solve the above technical problems.

[0006] In a first aspect, the present application provides a high temperature resistant and odor-free asphalt composition, which comprises the following components in parts by weight: 90-99 parts of asphalt and 1-10 parts of an odor-free agent, wherein the odor-free agent is composed of ricinoleic acid zinc grease, a porous dispersant and activated zinc powder.

[0007] In a preferred embodiment, the deodorant comprises the following components in parts by weight: 55-70 parts of ricinoleic acid zinc grease, 20-40 parts of porous dispersant and 5-10 parts of activated zinc powder.

[0008] In a preferred embodiment, the porous dispersant is any one of alumina, ultrafine activated carbon and 4A molecular sieve or a mixture of several of them in any proportion.

[0009] In a preferred embodiment, the alumina is prepared by calcination and activation at 500°C.

[0010] In a preferred embodiment, the asphalt is road petroleum asphalt, SBS modified asphalt or rubber powder modified asphalt.

[0011] In a second aspect, the present application provides a method for preparing a high temperature resistant and odorless asphalt composition, the method comprising the following steps:

[0012] S1, mixing the porous dispersant and the activated zinc powder and stirring for 30-60 minutes to obtain a first mixture;

[0013] S2, heating the first mixture to 80-100° C., adding ricinoleic acid zinc grease to the first mixture, stirring for 6-12 hours, and standing at room temperature for 24-48 hours to obtain a deodorizing agent;

[0014] S3. Weigh 90-99 parts of asphalt and 1-10 parts of deodorant, and mix the asphalt and the deodorant to obtain an asphalt composition.

[0015] In a preferred embodiment, the method for preparing a high temperature resistant and odorless asphalt composition provided in the present application further comprises the following steps:

[0016] S4. The volatile gases mixed and stirred for 2 h, 12 h and 24 h in step S3 are collected by a gas collector, and the concentrations of H2S, SO2, CO and NH3 are detected in the collected gases.

[0017] In a preferred embodiment, the method for preparing a high-temperature resistant and odor-free asphalt composition provided in the present application, in step S1, further includes: weighing 20-40 parts of a porous dispersant and 5-10 parts of activated zinc powder, mixing the porous dispersant and the activated zinc powder and stirring for 30-60 minutes to obtain a first mixture.

[0018] In a preferred embodiment, the method for preparing a high-temperature resistant and odor-free asphalt composition provided in the present application further includes, in step S2: heating the first mixture to 80-100°C, adding 55-70 parts of ricinoleic acid zinc grease to the first mixture, stirring for 6-12 hours, and standing at room temperature for 24-48 hours to obtain a deodorizer.

[0019] In a preferred embodiment, the method for preparing a high-temperature resistant and odor-free asphalt composition provided in the present application further includes, in step S3: weighing 90-99 parts of asphalt and 1-10 parts of odor-free agent, mixing and stirring the asphalt and the odor-free agent at 150-180°C for 30 minutes to obtain an asphalt composition.

[0020] The high temperature resistant and odorless asphalt composition and preparation method thereof provided in the present application have the following beneficial effects:

[0021] (1) Significantly improved high temperature resistance: By adopting a deodorant with specific components (zinc ricinoleate grease, porous dispersant and activated zinc powder), the asphalt composition of the present application significantly improves its high temperature performance while maintaining an effective deodorizing function, effectively avoiding the problem of damage to the high temperature performance of asphalt that may be caused by traditional liquid deodorizers.

[0022] (2) Excellent deodorizing effect: The ricinoleic acid zinc grease in the deodorizer has a highly efficient deodorizing function and can effectively remove the odor components in asphalt. Combined with the excellent dispersing properties of the porous dispersant, the deodorizer can be more evenly distributed in the asphalt, improving the deodorizing efficiency.

[0023] (3) Enhanced asphalt performance: The introduction of porous dispersants (such as alumina, ultrafine activated carbon, 4A molecular sieve) not only enhances the dispersibility of asphalt, but also may improve the physical and mechanical properties of asphalt to a certain extent, such as enhancing anti-aging properties and improving toughness.

[0024] (4) Environmental protection and safety: The selected materials are all environmentally friendly and do not contain harmful substances, which reduces the risk of environmental pollution during construction and use and improves safety of use.

[0025] (5) Wide range of applications: The composition is suitable for various types of asphalt, including road petroleum asphalt, SBS modified asphalt and rubber powder modified asphalt, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings:

[0027] Figure 1 The present invention is a flow chart of a method for preparing a high temperature resistant and odorless asphalt composition according to the present application. DETAILED DESCRIPTION

[0028] The present application will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It should also be noted that, for ease of description, only the parts related to the relevant invention are shown in the accompanying drawings.

[0029] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0030] In the first aspect, the present application provides a high temperature resistant and odor-free asphalt composition, which comprises the following components in parts by weight: 90-99 parts of asphalt and 1-10 parts of odor-free agent, wherein the odor-free agent comprises the following components in parts by weight: 55-70 parts of ricinoleic acid zinc grease, 20-40 parts of porous dispersant and 5-10 parts of activated zinc powder.

[0031] Preferably, the porous dispersant is any one of alumina, ultrafine activated carbon and 4A molecular sieve or a mixture of several of them in any proportion. The alumina is prepared by calcining and activating at a high temperature of 500°C.

[0032] Preferably, the asphalt is road petroleum asphalt of different grades, SBS modified asphalt or rubber powder modified asphalt.

[0033] Figure 1 A flow chart showing the preparation method of the high temperature resistant and odorless asphalt composition of the present application is shown, Figure 1 As shown, in the second aspect, the present application provides a method for preparing a high temperature resistant and odorless asphalt composition, the method comprising the following steps:

[0034] S1, weighing 20-40 parts of a porous dispersant and 5-10 parts of activated zinc powder, mixing the porous dispersant and the activated zinc powder and stirring for 30-60 minutes to obtain a first mixture;

[0035] S2, after heating the first mixture to 80-100° C., adding 55-70 parts of ricinoleic acid zinc grease to the first mixture, stirring for 6-12 hours, and standing at room temperature for 24-48 hours to obtain a deodorizing agent;

[0036] S3. Weigh 90-99 parts of asphalt and 1-10 parts of deodorant, mix and stir the asphalt and the deodorant at 150-180° C. for 30 minutes to obtain an asphalt composition.

[0037] S4. The volatile gases mixed and stirred for 2 h, 12 h and 24 h in step S3 are collected by a gas collector, and the concentrations of H2S, SO2, CO and NH3 are detected in the collected gases.

[0038] Example 1

[0039] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0040] a. Mix 30% by weight of aluminum oxide and 8% of activated zinc powder and stir for 30 minutes, then heat to 80° C., add 62% by weight of ricinoleic acid zinc grease, stir for 10 hours, and leave at room temperature for 36 hours to prepare a deodorant.

[0041] b. Mix 5% of the deodorant and 95% of 70A petroleum asphalt at a weight ratio at 150°C and stir for 30 minutes.

[0042] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0043]

[0044] From the above table, it can be seen that by adding 5% of the deodorant to 70A petroleum asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentration of H2S, NH3, SO2 and CO in the volatile gas, and the 2h sampling and the non-addition of the deodorant are reduced by about 47.2%, 35.2%, 64.0% and 30.6% respectively, and the softening point of the asphalt composition is increased from 47.4℃ to 49.8℃, and the 60℃ dynamic viscosity is also increased from 278Pa.s to 335Pa., showing better high temperature performance. The 12h sampling and the non-addition of the deodorant are reduced by about 46.6%, 39.7%, 66.3% and 28.5% respectively, and the softening point of the asphalt composition is increased from 47.4℃ to 49.5℃, and the 60℃ dynamic viscosity is also increased from 278Pa.s to 330Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 49.2%, 37.1%, 65.1% and 31.5 respectively. The softening point of the asphalt composition increased from 47.4℃ to 49.7℃, and the 60℃ dynamic viscosity increased from 278Pa.s to 338Pa.s, showing better high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0045] Comparative Example 1

[0046] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0047] a. Mix 20% by weight of aluminum oxide and 10% of activated zinc powder and stir for 60 minutes, then heat to 90° C., add 70% by weight of ricinoleic acid zinc grease, stir for 6 hours, and leave at room temperature for 24 hours to prepare a deodorant.

[0048] b. Mix 10% of the deodorant and 90% of 70A petroleum asphalt at a weight ratio at 180°C and stir for 30 minutes.

[0049] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0050]

[0051] From the above table, it can be seen that by adding 10% of the deodorant to 70A petroleum asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentration of H2S, NH3, SO2 and CO in the volatile gas, and the 2h sampling and the non-addition of the deodorant are reduced by about 55.72%, 33.72%, 67.38 and 28.18% respectively. In addition, the softening point of the asphalt composition is increased from 47.7℃ to 50.1℃, and the 60℃ dynamic viscosity is also increased from 279Pa.s to 345Pa.s, indicating that the high temperature performance of the asphalt composition is enhanced. The 12h sampling and the non-addition of the deodorant are reduced by about 54.23%, 33.02%, 68.98% and 31.18% respectively, the softening point of the asphalt composition is increased from 47.7℃ to 50.3℃, and the 60℃ dynamic viscosity is also increased from 279Pa.s to 350Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 56.22%, 34.18%, 71.12 and 30.25% respectively. The softening point of the asphalt composition increased from 47.7℃ to 49.7℃, and the 60℃ dynamic viscosity also increased from 279Pa.s to 358Pa.s, showing good high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0052] Comparative Example 2

[0053] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0054] a. Mix 40% by weight of aluminum oxide and 5% of activated zinc powder and stir for 45 minutes, then heat to 100° C., add 55% by weight of ricinoleic acid zinc grease, stir for 12 hours, and leave to stand at room temperature for 48 hours to prepare a deodorant.

[0055] b. Mix 1% by weight of deodorant and 99% by weight of 70A petroleum asphalt at 165°C and stir for 30 minutes.

[0056] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0057]

[0058] From the above table, it can be seen that by adding 1% of the deodorant to 70A petroleum asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentration of H2S, NH3, SO2 and CO in the volatile gas, and the 2h sampling and the non-addition of the deodorant are reduced by about 31.98%, 37.98%, 43.26% and 25.60% respectively. In addition, the softening point of the asphalt composition is increased from 47.7℃ to 49.1℃, and the 60℃ dynamic viscosity is also increased from 277Pa.s to 321Pa.s, indicating that the high temperature performance of the asphalt composition is enhanced. The 12h sampling and the non-addition of the deodorant are reduced by about 30.46%, 36.40%, 38.76% and 28.71% respectively, the softening point of the asphalt composition is increased from 47.7℃ to 49.5℃, and the 60℃ dynamic viscosity is also increased from 277Pa.s to 330Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 35.03%, 37.75%, 44.38% and 27.75% respectively. The softening point of the asphalt composition increased from 47.7℃ to 49.5℃, and the 60℃ dynamic viscosity also increased from 277Pa.s to 329Pa.s, showing better high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0059] Example 2

[0060] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0061] a. Mix 30% by weight of ultrafine activated carbon and 8% of activated zinc powder and stir for 30 minutes, then heat to 80° C., add 62% by weight of ricinoleic acid zinc grease, stir for 10 hours, and leave at room temperature for 36 hours to prepare a deodorizer.

[0062] b. Mix 5% of the deodorant and 95% of the SBS modified asphalt at a weight ratio at 150° C. and stir for 30 minutes.

[0063] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0064]

[0065] From the above table, it can be seen that by adding 5% of the deodorant to the SBS modified asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentration of H2S, NH3, SO2 and CO in the volatile gas, and the 2h sampling and the non-addition of the deodorant are reduced by about 49.85%, 38.97%, 55.76% and 27.73% respectively. In addition, the softening point of the asphalt composition is increased from 72.8℃ to 76.3℃, and the 60℃ dynamic viscosity is also increased from 5768Pa.s to 6340Pa.s, indicating that the high temperature performance of the asphalt composition has been enhanced. The 12h sampling and the non-addition of the deodorant are reduced by about 52.55%, 39.38%, 55.04% and 29.38% respectively, the softening point of the asphalt composition is increased from 72.8℃ to 77.1℃, and the dynamic viscosity is also increased from 5768Pa.s to 6423Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 48.65%, 38.97%, 56.83% and 28.44% respectively. The softening point of the asphalt composition increased from 72.8℃ to 75.9℃, and the dynamic viscosity increased from 5768Pa.s to 6435Pa.s, showing better high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0066] Comparative Example 3

[0067] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0068] a. Mix 20% by weight of ultrafine activated carbon and 10% of activated zinc powder and stir for 60 minutes, heat to 90° C., add 70% by weight of ricinoleic acid zinc grease, stir for 6 hours, and leave at room temperature for 24 hours to prepare a deodorizer.

[0069] b. Mix 10% of the deodorant and 90% of the SBS modified asphalt at a weight ratio at 180°C and stir for 2 hours.

[0070] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0071]

[0072]

[0073] From the above table, it can be seen that by adding 10% of the deodorant to the SBS modified asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentration of H2S, NH3, SO2 and CO in the volatile gas, and the 2h sampling and the non-addition of the deodorant are reduced by about 54.71%, 44.62%, 66.23% and 29.23% respectively. In addition, the softening point of the asphalt composition is increased from 73°C to 78.3°C, and the 60°C dynamic viscosity is also increased from 5880Pa.s to 6839Pa.s, indicating that the high temperature performance of the asphalt composition has been enhanced. The 12h sampling and the non-addition of the deodorant are reduced by about 56.18%, 43.20%, 65.23% and 30.16% respectively, the softening point of the asphalt composition is increased from 73°C to 78.1°C, and the dynamic viscosity is also increased from 5880Pa.s to 6829Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 54.41%, 45.64%, 65.89% and 30.63% respectively. The softening point of the asphalt composition increased from 73°C to 78.3°C, and the dynamic viscosity increased from 5880Pa.s to 6931Pa.s, showing better high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0074] Comparative Example 4

[0075] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0076] a. Mix 40% by weight of ultrafine activated carbon and 5% of activated zinc powder and stir for 45 minutes, then heat to 100° C., add 55% by weight of ricinoleic acid zinc grease, stir for 12 hours, and leave to stand at room temperature for 48 hours to prepare a deodorizer.

[0077] b. Mix 1% deodorant and 99% SBS modified asphalt at a weight ratio at 165°C and stir for 2 hours.

[0078] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0079]

[0080] From the above table, it can be seen that by adding 1% of the deodorant to the SBS modified asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentration of H2S, NH3, SO2 and CO in the volatile gas, and the 2h sampling and the non-addition of the deodorant are reduced by about 40.06%, 39.63%, 48.32% and 27.11% respectively. In addition, the softening point of the asphalt composition is increased from 72.8℃ to 76.1℃, and the 60℃ dynamic viscosity is also increased from 5738Pa.s to 6233Pa.s, indicating that the high temperature performance of the asphalt composition has been enhanced. The 12h sampling and the non-addition of the deodorant are reduced by about 41.25%, 40.25%, 46.98% and 25.87% respectively, the softening point of the asphalt composition is increased from 72.8℃ to 76.3℃, and the dynamic viscosity is also increased from 5738Pa.s to 6258Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 40.65%, 38.17%, 46.31% and 25.37% respectively. The softening point of the asphalt composition increased from 72.8℃ to 75.8℃, and the dynamic viscosity also increased from 5738Pa.s to 6189Pa.s, showing better high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0081] Example 3

[0082] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0083] a. Mix 30% by weight of activated alumina and 8% of activated zinc powder and stir for 2 hours, then heat to 80° C., add 62% by weight of ricinoleic acid zinc grease, stir for 10 hours, and leave at room temperature for 36 hours to prepare a deodorant.

[0084] b. Mix 5% of the deodorizer and 95% of the rubber powder modified asphalt at a weight ratio at 150°C and stir for 30 minutes.

[0085] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0086]

[0087] From the above table, it can be seen that by adding 5% of the deodorant to the rubber powder modified asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentrations of H2S, NH3, SO2 and CO in the volatile gas, which are reduced by about 56.79%, 36.53%, 63.86 and 26.38%, respectively. In addition, the softening point of the asphalt composition is increased from 65.3°C to 68.9°C, and the 60°C dynamic viscosity is also increased from 3878Pa.s to 4320Pa.s, indicating that the high temperature performance of the asphalt composition has been enhanced. The 12h sampling and the sample without adding the deodorant were reduced by about 58.55%, 34.25%, 63.48% and 25.13%, respectively, the softening point of the asphalt composition was increased from 65.3°C to 68.5°C, and the dynamic viscosity was also increased from 3878Pa.s to 4330Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 56.26%, 36.99%, 63.10% and 28.89% respectively. The softening point of the asphalt composition increased from 65.3℃ to 68.7℃, and the dynamic viscosity increased from 3878Pa.s to 4237Pa.s, showing better high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0088] Comparative Example 5

[0089] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0090] a. Mix 20% by weight of activated alumina and 10% of activated zinc powder and stir for 60 minutes, then heat to 90° C., add 70% by weight of ricinoleic acid zinc grease, stir for 6 hours, and leave at room temperature for 24 hours to prepare a deodorant.

[0091] b. Mix 10% of the deodorant and 90% of the rubber powder modified asphalt in a weight ratio at 180°C and stir for 30 minutes.

[0092] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0093]

[0094] From the above table, it can be seen that by adding 10% of the deodorant to the rubber powder modified asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentration of H2S, NH3, SO2 and CO in the volatile gas, and the 2h sampling is reduced by about 66.13%, 45.43%, 73.24% and 29.60% respectively. In addition, the softening point of the asphalt composition is increased from 65.5℃ to 70.2℃, and the 60℃ dynamic viscosity is also increased from 3990Pa.s to 4523Pa.s, indicating that the high temperature performance of the asphalt composition has been enhanced. The 12h sampling is reduced by about 66.45%, 46.99%, 74.44% and 27.86% respectively compared with the non-addition of the deodorant, the softening point of the asphalt composition is increased from 65.5℃ to 70.2℃, and the dynamic viscosity is also increased from 3990Pa.s to 4563Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 66.77%, 46.77%, 73.76% and 29.60% respectively. The softening point of the asphalt composition increased from 65.5℃ to 70.4℃, and the dynamic viscosity also increased from 3990Pa.s to 4532Pa.s, showing better high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0095] Comparative Example 6

[0096] The method for preparing a high temperature resistant and odorless asphalt composition of the present invention comprises the following steps:

[0097] a. Mix 40% by weight of activated alumina and 5% of activated zinc powder and stir for 45 minutes, then heat to 100° C., add 55% by weight of ricinoleic acid zinc grease, stir for 12 hours, and leave at room temperature for 48 hours to prepare a deodorant.

[0098] b. Mix 1% of the deodorizer and 99% of the rubber powder modified asphalt at a weight ratio at 165°C and stir for 30 minutes.

[0099] c. Place the gas collector on the top of the tank to collect the volatile gases after stirring for 2h, 12h and 24h. The collected gases are tested for concentration and technical parameters of H2S, SO2, CO and NH3. The results are shown in the following table.

[0100]

[0101] From the above table, it can be seen that by adding 1% of the deodorant to the rubber powder modified asphalt, the high temperature resistant deodorant asphalt composition prepared by the present invention significantly reduces the concentration of H2S, NH3, SO2 and CO in the volatile gas, and the 2h sampling and the non-addition of the deodorant are reduced by about 47.39%, 33.41%, 53.22% and 24.33% respectively. In addition, the softening point of the asphalt composition is increased from 65.2℃ to 66.8℃, and the 60℃ dynamic viscosity is also increased from 3870Pa.s to 4013Pa.s, indicating that the high temperature performance of the asphalt composition is enhanced. The 12h sampling and the non-addition of the deodorant are reduced by about 45.79%, 31.59%, 51.93% and 24.82% respectively. The softening point of the asphalt composition is increased from 65.2℃ to 66.9℃, and the dynamic viscosity is also increased from 3870Pa.s to 4016Pa.s, showing better high temperature performance. The 24h sampling and the sample without adding the deodorizer were reduced by about 45.87%, 32.27%, 51.75% and 26.52% respectively. The softening point of the asphalt composition increased from 65.2℃ to 66.9℃, and the dynamic viscosity also increased from 3870Pa.s to 3999Pa.s, showing better high temperature performance. In summary, this embodiment not only effectively removes the odor of asphalt, but also the deodorizer has basically no attenuation within 24 hours, and the effect is significant. It also effectively improves the high temperature resistance and physical properties of asphalt, showing excellent deodorization and modification effects.

[0102] In summary, the asphalt composition prepared by the present invention can suppress the smoke generated by the high-temperature process and disperse the gas reaction components in the porous material, which not only greatly improves the reaction efficiency and has a long-lasting effect, but also the inorganic porous dispersed material as a filler can effectively improve the high-temperature performance of the asphalt.

[0103] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the above invention concept. For example, the above features are replaced with the technical features with similar functions disclosed in this application (but not limited to) by each other to form a technical solution.

Claims

1. A high temperature resistant and odorless asphalt composition, characterized in that: The asphalt composition comprises the following components in parts by weight: 90-99 parts of asphalt and 1-10 parts of deodorant, wherein the deodorant consists of ricinoleic acid zinc grease, porous dispersant and activated zinc powder.

2. A high temperature resistant and odorless asphalt composition according to claim 1, characterized in that: The deodorant comprises the following components in parts by weight: 55-70 parts of ricinoleic acid zinc grease, 20-40 parts of porous dispersant and 5-10 parts of activated zinc powder.

3. A high temperature resistant and odorless asphalt composition according to claim 2, characterized in that: The porous dispersant is any one of aluminum oxide, ultrafine activated carbon and 4A molecular sieve or a mixture of several of them in any proportion.

4. A high temperature resistant and odorless asphalt composition according to claim 3, characterized in that: The alumina is prepared by calcining and activating at a high temperature of 500°C.

5. The high temperature resistant and odorless asphalt composition according to claim 1, characterized in that: The asphalt is road petroleum asphalt, SBS modified asphalt or rubber powder modified asphalt.

6. A method for preparing a high temperature resistant and odorless asphalt composition according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, mixing the porous dispersant and the activated zinc powder and stirring for 30-60 minutes to obtain a first mixture; S2, heating the first mixture to 80-100° C., adding ricinoleic acid zinc grease to the first mixture, stirring for 6-12 hours, and standing at room temperature for 24-48 hours to obtain a deodorizing agent; S3. Weigh 90-99 parts of asphalt and 1-10 parts of the deodorant, and mix the asphalt and the deodorant to obtain an asphalt composition.

7. The method for preparing a high temperature resistant and odorless asphalt composition according to claim 6, characterized in that: The following steps are also included: S4. The volatile gases mixed and stirred for 2 h, 12 h and 24 h in step S3 are collected by a gas collector, and the concentrations of H2S, SO2, CO and NH3 are detected in the collected gases.

8. The method for preparing a high temperature resistant and odorless asphalt composition according to claim 6, characterized in that: In step S1, the method further includes: weighing 20-40 parts of a porous dispersant and 5-10 parts of activated zinc powder, mixing the porous dispersant and the activated zinc powder and stirring them for 30-60 minutes to obtain a first mixture.

9. The method for preparing a high temperature resistant and odorless asphalt composition according to claim 6, characterized in that: In step S2, it also includes: heating the first mixture to 80-100° C., adding 55-70 parts of ricinoleic acid zinc grease to the first mixture, stirring for 6-12 hours, and standing at room temperature for 24-48 hours to obtain a deodorizing agent.

10. The method for preparing a high temperature resistant and odorless asphalt composition according to claim 6, characterized in that: In step S3, it also includes: weighing 90-99 parts of asphalt and 1-10 parts of the deodorant, mixing the asphalt and the deodorant at 150-180° C. and stirring for 30 minutes to obtain an asphalt composition.