Powder coating bonding process

By heating the powder coating foundation powder in the powder coating Binding process and using hot air dispersed pigments for uniform bonding, the problems of difficult temperature control and larger powder particle size in the existing technology are solved, and the efficiency and product quality of the Binding are improved .

CN118909481APending Publication Date: 2024-11-08ZHENGZHOU JIANUO IND CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411075411.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing powder coating bonding process has problems such as difficult to control temperature, low bonding rate, larger powder particle size, high cost and low production efficiency, resulting in poor product stability and reduced yield.

Method used

By heating the powder coating foundation in a Bonding pot to a temperature close to the softening point, heating the pigment with a heating tank or hot air and dispersing it, gradually adding it to the Bonding pot, and making the pigment evenly bond to the base powder by stirring to avoid Sticking and clumping.

Benefits of technology

It realizes efficient and stable powder coating bonding, improves the bonding rate and production efficiency, reduces the phenomenon of powder sticking, and ensures the product's appearance stability and high quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909481A_ABST
    Figure CN118909481A_ABST
Patent Text Reader

Abstract

The invention is applicable to the technical field of powder coatings, and provides a powder coating bonding process, which comprises the following steps: S1, bottom powder heating: adding powder coating bottom powder into a bonding pot, setting the temperature required to be heated according to the glass transition temperature of the powder coating bottom powder, and enabling the temperature to be 1-2 DEG C lower than the traditional bonding temperature, continuously raising the temperature through a water jacket on the side wall of the bonding pot, setting the rotating speed of a paddle, heating while stirring, lowering the rotating speed of the paddle after the temperature is raised to a constant temperature, keeping the constant temperature, and continuously stirring; s2, the pigment is heated; and S3, mixing: adding the pigment, continuously mixing for 60-600 seconds, introducing cold water after mixing, cooling to 40 DEG C, and discharging. According to the invention, the powder is prevented from sticking to a pan, the bonding is improved, the bonding window is wider, the pigment bonding rate is greatly improved, and the caking phenomenon of the powder base powder is reduced; and one-time success of bonding is realized, and the product percent of pass and the production efficiency are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder coatings, in particular to a powder coating bonding process. Background Art

[0002] Powder coating refers to a powder coating that contains a certain proportion of metal effect pigments such as aluminum powder, copper powder, pearl powder, glass powder, etc. in its product ingredients, and its paint film has a certain metal surface effect, close to or reaching the effect of current metal paint. Powder coating is deeply loved by users due to its good decorative properties. With the advancement of the current paint-to-powder conversion, the market demand for powder coating is increasing. However, the current problem with powder coating is that the pigment and the powder coating base powder have different charges, and the powder application rate is different during spraying, resulting in the separation of metal powder and base powder, resulting in surface flowery, color difference of workpieces, poor batch stability, and silver powder accumulation and spitting to form surface particles. These problems have seriously affected the promotion and use of powder coating.

[0003] There are two main solutions at present: one is to coat the pigment with certain organic matter so that it has a similar charge as the powder coating base powder, so as to achieve a uniform powder coating effect, which is the so-called bonding-free pigment on the market; the other is through the process of thermal bonding, using a bonding machine, and its general process flow is to pour the powder coating base powder into the bonding pot, and heat the powder coating base powder through the hot water jacket on the pot wall and the rotating friction of the paddle blades. When the base powder reaches or exceeds the softening point temperature, the pigment is added to make the pigment and the base powder bond together, so as to achieve a uniform and consistent ratio of pigment to base powder.

[0004] The first type of non-bonding pigment has a certain improvement effect on low-content powder coatings, but it is not ideal for high-content powder coatings. The reason is that the organic coating rate of the pigment is unstable, and the charge of the organic matter is also different from that of the base powder. Therefore, the high-end powder coatings on the market are still mainly based on the second bonding process.

[0005] The existing bonding process has the following problems:

[0006] 1. It is difficult to control the bonding temperature during bonding. If the temperature is too low, the bonding rate will be low. If the temperature is too high, the pot will stick, resulting in product scrapping. It is difficult to achieve a high bonding rate, and the batch stability is also poor.

[0007] 2. After reaching the softening point, not only the metal powder and the base powder will stick together, but the base powders will also stick together, causing the powder particle size to become coarser, and even forming large-particle powder agglomerates, reducing the yield rate;

[0008] 3. Due to the irregularity of the bonding powder agglomerates, the fluidity of the dry powder deteriorates, and even affects the leveling of the spray powder and the paint film surface;

[0009] 4. In order to improve the bonding efficiency and increase the temperature of the base powder to avoid agglomeration and sticking to the pan, some bonding additives need to be added, which also increases the bonding cost;

[0010] 5. If bonding is unsuccessful once, it needs to be bonded again. The pigment will be broken repeatedly, which will also change the original color. Multiple rework is time-consuming and labor-intensive, which greatly affects production efficiency.

[0011] Therefore, the present invention proposes a powder coating bonding process. Summary of the invention

[0012] The object of the present invention is to provide a powder coating bonding process to solve the problems existing in the existing bonding process in the above-mentioned background technology.

[0013] To achieve the above object, the present invention provides the following technical solution: a powder coating bonding process, the powder coating bonding process comprising the following steps:

[0014] S1, base powder heating:

[0015] Add the powder coating base powder into the bonding pot, set the required heating temperature according to the glass transition temperature of the powder coating base powder, which is 1-2°C lower than the traditional bonding temperature, and continue to heat up through the water jacket on the side wall of the bonding pot. Set the paddle speed, stir and heat at the same time, and after reaching a constant temperature, reduce the paddle speed, maintain a constant temperature, and continue stirring;

[0016] S2, heating the pigment:

[0017] Set the heating temperature of the pigment according to the particle size and quality of the pigment. When the pigment reaches the set temperature, add it into the bonding machine.

[0018] S3, Mixing:

[0019] After adding the pigment, continue mixing for 60-600 seconds. After mixing is completed, cool it down to 40°C with cold water and then discharge the material.

[0020] Preferably, there are two operating modes of S2:

[0021] The first method is to add the pigment to be heated into the heating tank, and heat the pigment through the heating tank. The heating temperature is set according to the particle size and quality of the pigment. The set temperature is 60℃-200℃. After the pigment reaches the set temperature, it naturally falls to the base powder in the bonding pot through the insulation pipe.

[0022] The second method is to heat the pigment with hot air and disperse the pigment. The specific steps are: add the pigment into the heating tank, pump in hot air with an air pump to heat it. The hot air temperature is set at 60℃-110℃, and then sucked into the bonding pot by a Venturi powder pump to disperse it.

[0023] Preferably, the mass percentages of the base powder and the pigment are as follows:

[0024] Base powder 80-99%, pigment 1-20%.

[0025] Preferably, the pigment is one or more of metal powder, organic coated metal pigment and powder coating.

[0026] Preferably, the metal powder is one or more of aluminum powder, copper powder, zinc powder, stainless steel powder, pearl powder and glass powder.

[0027] Preferably, the base powder is a powder base material made of acrylic polyester or epoxy resin as a main film-forming substance.

[0028] Preferably, the powder coating bonding process is completed by bonding equipment, which includes a pigment heating device and a bonding machine; a water jacket is provided on the outside of the bonding machine, paddles are provided on the inside of the bonding machine, and a bonding pot is provided on the inside of the bonding machine.

[0029] Preferably, the pigment heating device includes a heating tank, which is arranged above the bonding machine. A Venturi powder pump is provided at the bottom of the heating tank. The output end of the Venturi powder pump is connected to the interior of the bonding machine through a pipeline. A pressure-stabilizing gas tank and an air pump are provided on one side of the Venturi powder pump. The input end of the air pump is connected to the pressure-stabilizing gas tank, and the output end of the air pump is connected to the Venturi powder pump through a pipeline. An air heating component is provided on the pipeline sleeve between the air pump and the Venturi powder pump. The air heating component is electrically connected to the first system control box, and an air vent pipe is passed through the top surface of the bonding machine.

[0030] Preferably, the pigment heating device comprises a storage tank, which is arranged above the bonding machine, an insulation pipe is provided between the bottom of the storage tank and the bonding machine, the heating tank is electrically connected to the first system control box, and the insulation pipe is connected to a discharge valve.

[0031] The present invention has at least the following beneficial effects:

[0032] The powder coating bonding process provided by the present invention can prevent powder from sticking to the pan, improve bonding, have a wider bonding window, greatly improve the pigment bonding rate, and reduce the agglomeration of powder base powder; achieve one-time success in bonding, greatly improve the product qualification rate and production efficiency, and the powder coating after bonding has a stable appearance, no color difference, and high quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the effect diagram of powder coating bonding;

[0034] Figure 2 A structural diagram of a bonding device according to the second method of S2 of the present invention;

[0035] Figure 3 This is a structural diagram of the first method bonding device of S2 of the present invention.

[0036] In the accompanying drawings: 1. bonding machine; 2. paddle; 3. heating tank; 4. pressure-stabilizing air storage tank; 5. venturi powder pump; 6. air release pipe; 7. first system control box; 8. air heating assembly; 9. water jacket; 10. insulation pipe; 11. air pump; 12. discharge valve; 13. storage tank; 14. second system control box. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The present invention provides a powder coating bonding process, comprising the following steps:

[0039] S1, base powder heating:

[0040] Add the powder coating base powder into the bonding pot, set the required heating temperature according to the glass transition temperature of the powder coating base powder, which is 1-2°C lower than the traditional bonding temperature, and continue to heat up through the water jacket on the side wall of the bonding pot. Set the paddle speed, stir and heat at the same time, and after reaching a constant temperature, reduce the paddle speed, maintain a constant temperature, and continue stirring;

[0041] S2, heating the pigment:

[0042] Set the heating temperature of the pigment according to the particle size and quality of the pigment. When the pigment reaches the set temperature, add it into the bonding machine.

[0043] S3, Mixing:

[0044] After adding the pigment, continue mixing for 60-600 seconds. After mixing is completed, cool it down to 40°C with cold water and then discharge the material.

[0045] Among them, the pigment is one or more of metal powder, organic coated metal pigment and powder coating; the metal powder is one or more of aluminum powder, copper powder, zinc powder, stainless steel powder, pearl powder and glass powder; the base powder is a powder base material made of acrylic polyester or epoxy resin as the main film-forming substance.

[0046] Among them, S2 has two operating modes:

[0047] The first method is to add the pigment to be heated into the heating tank, and heat the pigment through the heating tank. The heating temperature is set according to the particle size and quality of the pigment. The set temperature is 60℃-200℃. After the pigment reaches the set temperature, it naturally falls to the base powder in the bonding pot through the insulation pipe.

[0048] The second method is to heat the pigment with hot air and disperse the pigment. The specific steps are: add the pigment into the heating tank (no need to heat it in the heating tank), pump in hot air with an air pump to heat it. The hot air temperature is set at 60℃-110℃, and then sucked in by the Venturi powder pump and pumped into the bonding pot to disperse it.

[0049] The first method mentioned above is only applicable to metallic pigments; the second method is applicable to all pigments, especially those that melt and become sticky at high temperatures, or even those that require the addition of another type of powder coating. The problem it solves is to disperse the pigments that need to be heated while heating them with hot air, and to isolate the pigments from each other through air to prevent them from agglomerating when heated.

[0050] Among them, the mass percentages of base powder and pigment are as follows:

[0051] Base powder 80-99%, pigment 1-20%.

[0052] Based on the above technical solution, the present invention provides the following partial embodiments:

[0053] Example 1

[0054] A powder coating bonding process comprises the following steps:

[0055] S1, base powder heating:

[0056] Add the powder coating base powder into the bonding pot, set the heating temperature of the powder coating base powder at 59°C, pass 59°C water into the water jacket, continue to heat up through the water jacket on the side wall of the bonding pot, set the paddle speed at 32 Hz, stir and heat at the same time, after reaching a constant temperature, reduce the paddle speed to 30 Hz, keep the constant temperature, and continue stirring;

[0057] S2, heating the pigment:

[0058] Add the pigment to be heated into the heating tank, heat the pigment through the heating tank, set the temperature at 120℃, and when the pigment reaches the set temperature, it will naturally fall onto the base powder in the bonding pot through the insulation pipe;

[0059] S3, Mixing:

[0060] After adding the pigment, continue mixing for 100 seconds. After mixing is completed, cool it down to 40°C with cold water and then discharge the material.

[0061] Among them, the mass percentages of base powder and pigment are as follows:

[0062] 80% foundation powder, 20% pigment.

[0063] The pigment is a metallic pigment, specifically a mixture of aluminum powder and copper powder; the components of the base powder are as follows:

[0064] Polyester resin 300g, TGIC 23g, leveling agent 5g, brightener 4g, titanium dioxide 200g, benzoin 3g, ultramarine 0.5g.

[0065] Example 2

[0066] S1, base powder heating:

[0067] The following steps are involved:

[0068] S1, base powder heating:

[0069] Add the powder coating base powder into the bonding pot, set the heating temperature of the powder coating base powder at 65℃, pass 65℃ water into the water jacket, continue to heat up through the water jacket on the side wall of the bonding pot, set the paddle speed at 28 Hz, stir and heat at the same time, after reaching a constant temperature, reduce the paddle speed to 25 Hz, keep the constant temperature, and continue stirring;

[0070] S2, heating the pigment:

[0071] The pigment is heated by hot air and dispersed. The specific steps are as follows: add the pigment into the heating tank (no need to heat it in the heating tank), pump hot air into it by an air pump for heating, the temperature of the hot air is set at 100°C, and then sucked into the bonding pot by the Venturi powder pump to disperse it;

[0072] S3, Mixing:

[0073] After adding the pigment, continue mixing for 150 seconds. After mixing is completed, cool it down to 40°C with cold water and then discharge the material.

[0074] Among them, the mass percentages of base powder and pigment are as follows:

[0075] 90% foundation powder, 10% pigment.

[0076] Wherein, the pigment is an organic coated metal pigment; the components of the base powder are as follows:

[0077] Polyester resin 450g, TGIC 34g, leveling agent 5g, brightener 5g, benzoin 3g.

[0078] Example 3

[0079] The following steps are involved:

[0080] S1, base powder heating:

[0081] Add the powder coating base powder into the bonding pot, set the heating temperature of the powder coating base powder at 69°C, pass 69°C water into the water jacket, continue to heat up through the water jacket on the side wall of the bonding pot, set the paddle speed at 30 Hz, stir and heat at the same time, after reaching a constant temperature, reduce the paddle speed to 28 Hz, keep the constant temperature, and continue stirring;

[0082] S2, heating the pigment:

[0083] The pigment is heated by hot air and dispersed. The specific steps are as follows: add the pigment into the heating tank (no need to heat it in the heating tank), pump hot air into it with an air pump to heat it, the temperature of the hot air is set at 90°C, and then sucked into the bonding pot by the Venturi powder pump to disperse it;

[0084] S3, Mixing:

[0085] After adding the pigment, continue mixing for 120 seconds. After mixing is completed, cool it down to 40°C with cold water and then discharge the material.

[0086] Among them, the mass percentages of base powder and pigment are as follows:

[0087] Foundation powder 99%, pigment 1%.

[0088] Among them, the pigment is powder coating; the components of the base powder are as follows:

[0089] 200g epoxy resin, 200g polyester resin, 5g leveling agent, 5g brightener, 4g benzoin, 0.1g carbon black, 0.1g ultramarine, 5g barium sulfate.

[0090] The powder coating bonding process provided by the present invention is completed by a bonding device, and the bonding device includes a pigment heating device and a bonding machine 1.

[0091] A water jacket 9 is provided on the outside of the bonding machine 1, and a water inlet pipe and a water outlet pipe are provided on the side wall of the water jacket 9. A paddle 2 is provided inside the bonding machine 1, and the paddle 2 is connected through a rod shaft. The rod shaft passes through the bottom surface of the bonding machine 1 and extends to the outside. A pulley is connected to one end of the rod shaft located outside the bonding machine 1, and the pulley is connected to the motor through a belt.

[0092] There are two ways to set up the pigment heating device according to S2:

[0093] The first method is to heat the pigment in a heating tank. When the pigment reaches the set temperature, it naturally falls through the insulation tube onto the base powder in the bonding pot:

[0094] like Figure 3As shown, the pigment heating device includes a storage tank 13, which is arranged above the bonding machine 1. An insulation pipe 10 is provided between the bottom of the storage tank 13 and the bonding machine 1. The storage tank 13 is electrically connected to a second system control box 14, and the insulation pipe 10 is connected to a discharge valve 12.

[0095] When the pigment heating device is in use, the heating temperature of the storage tank 13 is first set through the second system control box 14. When heated to the set temperature, the material release valve 12 is opened, and the pigment naturally falls onto the base powder in the bonding pot through the insulation pipe 10.

[0096] The second method is to heat the pigment with hot air and disperse it:

[0097] like Figure 2 As shown, the pigment heating device includes a heating tank 3, which is arranged above the bonding machine 1. A venturi powder pump 5 is provided at the bottom of the heating tank 3. The output end of the venturi powder pump 5 is connected to the inside of the bonding machine 1 through a pipeline. A pressure-stabilizing gas storage tank 4 and an air pump 11 are provided on one side of the venturi powder pump 5. The input end of the air pump 11 is connected to the pressure-stabilizing gas storage tank 4, and the output end of the air pump 11 is connected to the venturi powder pump 5 through a pipeline. An air heating component 8 is provided on the pipeline sleeve between the air pump 11 and the venturi powder pump 5. The air heating component 8 is electrically connected to the first system control box 7. An air vent pipe 6 is passed through the top surface of the bonding machine 1.

[0098] When the pigment heating device is in use, pigment is added into the heating tank 3, air is pumped out of the pressure-stabilizing air tank 4 by the air pump 11, and heated by the air heating component 8. The temperature of the air heating component 8 is set by the first system control box 7, and the heated air is pumped into the bonding machine 1 through the Venturi sub-pump 5 to disperse the pigment.

[0099] The heat preservation pipe 10 and the output end pipe of the Venturi powder pump 5 of the above two types of equipment are extended to a position close to the top of the blade, so that the pigment can quickly contact the base powder when adding materials.

[0100] The difference between the present invention and the existing bonding process is:

[0101] The present invention only needs to heat the bonding base powder to a temperature close to the softening point of the base powder, but does not need to reach the softening point. Then, the pigment to be bonded is heated to a temperature higher than the softening point of the base powder, and is added to the bonding pot in batches. The pigment is stirred by blades to evenly distribute the pigment in the base powder. Since the temperature of the pigment is higher than the softening point of the base powder, when it contacts the powder base powder, it will transfer heat to the base powder, causing it to heat up to or even exceed the softening temperature. Since the base powder is only heated and softened on the surface in contact with the metal powder, the metal powder and the base powder can be fully bonded, and the theoretical value is close to 100%, and there is no bonding between the base powders. This method not only avoids the problem of sticking to the pot during bonding, but also basically eliminates the problem of powder agglomeration reducing the yield rate, and can achieve one-time success in bonding. The product qualification rate and production efficiency are greatly improved.

[0102] This solution has a simple equipment structure and does not require excessive investment. It can produce high-quality powder coatings based on existing bonding equipment. It has great economic significance for powder coating production.

[0103] Figure 1 This is the effect of powder coating bonding. The powder coating after bonding has a stable appearance, no color difference and high quality.

[0104] The above shows and describes the basic principles, main features and advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.

[0105] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A powder coating bonding process, characterized in that: The powder coating bonding process comprises the following steps: S1, base powder heating: Add the powder coating base powder into the bonding pot, set the required heating temperature according to the glass transition temperature of the powder coating base powder, which is 1-2°C lower than the traditional bonding temperature, and continue to heat up through the water jacket on the side wall of the bonding pot. Set the paddle speed, stir and heat at the same time, and after reaching a constant temperature, reduce the paddle speed, maintain a constant temperature, and continue stirring; S2, heating the pigment: Set the heating temperature of the pigment according to the particle size and quality of the pigment. When the pigment reaches the set temperature, add it into the bonding machine. S3, Mixing: After adding the pigment, continue mixing for 60-600 seconds. After mixing is completed, cool it down to 40°C with cold water and then discharge the material.

2. A powder coating bonding process according to claim 1, characterized in that: There are two modes of operation of S2: The first method is to add the pigment to be heated into the heating tank, and heat the pigment through the heating tank. The heating temperature is set according to the particle size and quality of the pigment. The set temperature is 60℃-200℃. After the pigment reaches the set temperature, it naturally falls to the base powder in the bonding pot through the insulation pipe. The second method is to heat the pigment with hot air and disperse the pigment. The specific steps are: add the pigment into the heating tank, pump in hot air with an air pump to heat it. The hot air temperature is set at 60℃-110℃, and then sucked into the bonding pot by a Venturi powder pump to disperse it.

3. A powder coating bonding process according to claim 2, characterized in that: The mass percentages of the base powder and the pigment are as follows: Base powder 80-99%, pigment 1-20%.

4. A powder coating bonding process according to claim 3, characterized in that: The pigment is one or more of metal powder, organic coated metal pigment and powder coating.

5. A powder coating bonding process according to claim 4, characterized in that: The metal powder is one or more of aluminum powder, copper powder, zinc powder, stainless steel powder, pearl powder and glass powder.

6. A powder coating bonding process according to claim 5, characterized in that: The base powder is a powder base material made of acrylic polyester or epoxy resin as a main film-forming substance.

7. A powder coating bonding process according to claim 6, characterized in that: The powder coating bonding process is completed by bonding equipment, which includes a pigment heating device and a bonding machine (1); a water jacket (9) is provided on the outside of the bonding machine (1), a paddle (2) is provided on the inside of the bonding machine (1), and a bonding pot is provided on the inside of the bonding machine (1).

8. A powder coating bonding process according to claim 7, characterized in that: The pigment heating device comprises a heating tank (3), wherein the heating tank (3) is arranged above the bonding machine (1), a venturi powder pump (5) is arranged at the bottom of the heating tank (3), the output end of the venturi powder pump (5) is connected to the inside of the bonding machine (1) through a pipeline, a pressure-stabilizing gas storage tank (4) and an air pump (11) are arranged on one side of the venturi powder pump (5), the input end of the air pump (11) is connected to the pressure-stabilizing gas storage tank (4), the output end of the air pump (11) is connected to the venturi powder pump (5) through a pipeline, an air heating component (8) is arranged on the pipeline between the air pump (11) and the venturi powder pump (5), and the air heating component (8) is electrically connected to a first system control box (7), and an air release pipe (6) is passed through the top surface of the bonding machine (1).

9. A powder coating bonding process according to claim 7, characterized in that: The pigment heating device comprises a storage tank (13), wherein the storage tank (13) is arranged above the bonding machine (1), and an insulation pipe (10) is provided between the bottom of the storage tank (13) and the bonding machine (1), the heating tank (3) is electrically connected to a second system control box (14), and the insulation pipe (10) is connected to a discharge valve (12).

Citation Information

Cited By

  • Metal powder coating and bonding process thereof

    CN121182248A