1, 5-diisocyanate pentane-polyurethane coating and preparation method thereof
High-performance 1,5-diisocyanate-polyurethane coating was prepared by combining vegetable oil polyols and 1,5-diisocyanate pentane, combined with ionic liquid catalysts and hydrophilic chain extenders, and solved the problem of The oil resource shortage and environmental pollution problems have been solved, and the performance improvement and industrial applicability of coatings have been achieved.
Patent Information
- Application Number
- CN202410945537.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The existing water-based polyurethane coatings rely on petroleum resources during the preparation process, resulting in resource shortages and environmental pollution, and insufficient material performance.
Using vegetable oil polyol combined with 1,5-diisocyanate pentane, 1,5-diisocyanate-polyurethane coating was prepared by ionic liquid catalyst and hydrophilic chain extender, reducing oil resource dependence and improving oil resources Material properties.
It improves the biocarbon content, reduces environmental pollution, solves the problem of petroleum resource shortage, and at the same time improves the adhesive properties and mechanical properties of the coating, which is suitable for industrial production.
Smart Images

Figure BDA0004945512790000031 
Figure BDA0004945512790000071 
Figure FDA0004945512780000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical engineering, and specifically relates to a 1,5-diisocyanatopentane-polyurethane coating and a preparation method thereof. Background Art
[0002] Polyurethane is a polymer with repeating structural units of carbamate segments made by the reaction of isocyanate and polyol. The traditional polyurethane system mainly uses two main raw materials: petrochemical polyether or polyester polyol and isocyanate. Polyurethane products are divided into two categories: foaming products and non-foaming products. Foaming products include soft, hard, and semi-hard polyurethane foam plastics; non-foaming products include coatings, adhesives, synthetic leather, elastomers, and elastic fibers. Polyurethane materials have excellent performance, a wide range of uses, and many types of products, among which polyurethane coatings are the most widely used.
[0003] In recent years, with the increase of people's environmental awareness and their concern for their own health, coupled with the strict requirements of environmental regulations on the emission of volatile organic compounds (VOC) and the content of harmful solvents, the application of polyurethane coatings containing solvents and organic fillers has been greatly restricted, prompting polyurethane coatings to develop in the direction of water-based, powdered and high solid content. Among them, water-based polyurethane coatings use water as a dispersion medium, and are highly valued by the coating industry because of their safety, non-toxicity, solvent-free volatilization, environmental friendliness, and good water resistance. The development of water-based polyurethane coatings has become one of the hot spots in the field of polyurethane coatings in recent years. However, the existing water-based polyurethane coatings mostly use petroleum as raw materials to prepare polyols, which requires the consumption of a large amount of petroleum resources, and the use of petroleum to prepare polyols has problems such as complex processes and serious pollution. Natural oils are currently recognized and the only renewable petroleum substitute, and among natural oils, vegetable oils have the most ideal performance. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a 1,5-diisocyanatopentane-polyurethane coating and a preparation method thereof, by introducing vegetable oil molecules into the polyurethane material using a ring-opening reagent of vegetable oil polyol, which can not only solve the problems of oil resource shortage and environmental pollution, but also increase the added value of vegetable oil products.
[0005] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] The first aspect of the present invention is to provide a 1,5-diisocyanatopentane-polyurethane coating, which comprises the following raw materials in parts by weight: 100 parts of vegetable oil polyol, 40-75 parts of isocyanate, 30-40 parts of organic solvent, 0.1-2 parts of ionic liquid catalyst, 10-20 parts of flame retardant, 10-30 parts of hydrophilic chain extender, 10-30 parts of neutralizer, and 20-40 parts of deionized water.
[0007] In some embodiments, the vegetable oil polyol is selected from at least one of olive oil polyol, peanut oil polyol, rapeseed oil polyol, cottonseed oil polyol, soybean oil polyol, coconut oil polyol, palm oil polyol, sesame oil polyol, corn oil polyol, and sunflower oil polyol; and the hydroxyl value of the vegetable oil polyol is 160-200 mgKOH / g.
[0008] Preferably, the vegetable oil polyol is soybean oil polyol.
[0009] It should be noted that the vegetable oil polyols can be selected from FH-3170 and FHB-195 (manufacturer: Zhangjiagang Feihang Technology Co., Ltd.).
[0010] In some embodiments, the isocyanate is 1,5-pentanediisocyanate; and the organic solvent is selected from at least one of acetone, ethyl acetate, dichloromethane, dichloroethane, chloroform, n-hexane, tetrahydrofuran, and carbon tetrachloride.
[0011] Preferably, the organic solvent is acetone.
[0012] In some embodiments, the ionic liquid catalyst is selected from at least one of a pyridine-type ionic liquid catalyst, an imidazole-type ionic liquid catalyst, and a long-chain fatty amine-type ionic liquid catalyst; the ionic liquid catalyst includes anions and cations.
[0013] It should be noted that the present invention selects an ionic liquid catalyst containing a tertiary amine and a quaternary ammonium salt structure because the tertiary amine structure in the catalyst can play a catalytic role in reducing the spatial position and activating the hydroxyl group, but the catalytic effect on the activity of isocyanate molecules is relatively low, and the quaternary ammonium structure can play an activation role by reacting with the oxygen in the isocyanate, further overcoming the problems of poor activity of the neutralizer in the polymerization reaction, low reaction rate and poor material performance caused by system inhomogeneity; and the quaternary ammonium N positive ion has a better effect of connecting 2 or 3 carbons with the tertiary amine N, so a pyridine-type ionic liquid catalyst, an imidazole-type ionic liquid catalyst or a long-chain fatty amine-type ionic liquid catalyst is selected.
[0014] In some embodiments, the anion is selected from Bronsted base, selected from at least one of dicyanamide, hexafluorophosphate, boron tetrafluoride, and bistrifluoromethanesulfonyl imide;
[0015] Preferably, the Bronsted base is dicyanamide.
[0016] In some embodiments, the cation is selected from at least one of the following structural formulas CA-1, CA-2, CA-3, CA-4, CA-5, CA-6, CA-8, CA-9, CB-1, CB-2, CB-3, CB-4, CB-5, CB-6, CB-7, CB-8, CB-9, and CB-10,
[0017]
[0018] Preferably, the cation in the ionic liquid catalyst is CB-5.
[0019] In some embodiments, the flame retardant is selected from at least one of tributyl phosphate, tri(2-ethylhexyl) phosphate, tri(2-chloroethyl) phosphate, tri(2,3-dichloropropyl) phosphate, tri(2,3-dibromopropyl) phosphate, flame retardant Pyrol99, toluene-diphenyl phosphate, tricresyl phosphate, triphenyl phosphate, (2-ethylhexyl)-diphenyl phosphate, bis(4-hydroxyphenyl)phenylphosphine oxide, and casein;
[0020] Preferably, the flame retardant is flame retardant Pyrol99.
[0021] The neutralizing agent is selected from at least one of triethylamine, dimethylethanolamine and N,N-dimethylcyclohexylamine.
[0022] In some embodiments, the hydrophilic chain extender is a dihydroxy half ester; the dihydroxy half ester is prepared from a triol and a dibasic acid anhydride; wherein the triol is glycerol, and the dibasic acid anhydride is selected from at least one of phthalic anhydride, 1,2-cyclohexanedicarboxylic anhydride, nadic anhydride, and cyclopentane-1,2-dicarboxylic anhydride.
[0023] It should be noted that the present invention uses a dihydroxy half ester prepared from a triol and a dibasic acid anhydride, which can introduce a cyclic structure into the polyurethane, thereby improving the mechanical properties of the material.
[0024] The second aspect of the present invention is to provide a method for preparing a 1,5-diisocyanate pentane-polyurethane coating, comprising the following steps:
[0025] S1: mixing and reacting vegetable oil polyol, isocyanate, organic solvent, flame retardant and ionic liquid catalyst to obtain a prepolymer mixture;
[0026] S2: adding a hydrophilic chain extender to the prepolymer mixture to react and obtain a polymer mixture;
[0027] S3: After the polymer mixture is cooled, a neutralizing agent is added, and then deionized water is added to emulsify the mixture to form a polyurethane emulsion;
[0028] S4: The polyurethane emulsion is obtained by removing the organic solvent through reduced pressure distillation.
[0029] In some embodiments, the mixed reaction temperature in S1 is 40-70°C, and the mixed reaction time is 1-3h; the reaction temperature in S2 is 40-70°C, and the reaction time is 2-5h; and the temperature is lowered to 20-30°C in S3.
[0030] The present invention has the following beneficial effects:
[0031] 1. The present invention uses vegetable oil polyols with specific hydroxyl values as raw materials, and is matched with isocyanates and ionic liquid catalysts from biomass. The formulation system and catalytic system can increase the content of biocarbon in the coating. The high biocarbon content can reduce environmental pollution and solve the problem of shortage of petroleum resources, thereby greatly increasing the added value of vegetable oil products.
[0032] 2. Compared with traditional polyurethane coatings, the 1,5-diisocyanate pentane-polyurethane coating prepared by the present invention not only has good bonding properties and mechanical properties, but also does not require the use of non-renewable resources such as petroleum, further reducing the production cost of the coating, and is suitable for industrial production. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below. The embodiments described are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.
[0034] Example 1
[0035] A preparation method of 1,5-diisocyanatopentane-polyurethane coating:
[0036] 100 parts of vegetable oil polyol FH-3170, 49 parts of 1,5-diisocyanatopentane, and 15 parts of flame retardant Pyrol99 were mixed in 30 parts of acetone, and 0.5 parts of imidazole type ionic liquid catalyst (anion is dicyanamide, cation is CB-5) was added, and the mixture was reacted at 50°C for 2h to obtain a prepolymer mixture;
[0037] Add 30 parts of a hydrophilic chain extender dihydroxy half ester (synthesized from glycerol and phthalic anhydride) to the prepolymer mixture, and react at 50° C. for 3 hours to obtain a polymer mixture;
[0038] The polymer mixture was cooled to 30°C and then 14 parts of a neutralizing agent triethylamine was added to neutralize it to neutrality. 30 parts of deionized water were added and emulsified at high speed to form a polyurethane emulsion. The polyurethane emulsion was distilled under reduced pressure to remove acetone to obtain a vegetable oil-based waterborne polyurethane coating.
[0039] Example 2
[0040] A preparation method of 1,5-diisocyanatopentane-polyurethane coating:
[0041] 100 parts of vegetable oil polyol FHB-195, 49 parts of 1,5-diisocyanatopentane, and 15 parts of flame retardant Pyrol99 were mixed in 30 parts of acetone, and 0.5 parts of imidazole type ionic liquid catalyst (anion is dicyanamide, cation is CB-5) was added, and the mixture was reacted at 50°C for 2h to obtain a prepolymer mixture;
[0042] Add 30 parts of a hydrophilic chain extender dihydroxy half ester (synthesized from glycerol and phthalic anhydride) to the prepolymer mixture, and react at 50° C. for 3 hours to obtain a polymer mixture;
[0043] The polymer mixture was cooled to 30°C and then 17 parts of a neutralizing agent, N,N-dimethylcyclohexylamine, was added to neutralize the mixture to neutrality. 30 parts of deionized water were added to form a polyurethane emulsion by high-speed shear emulsification. The polyurethane emulsion was distilled under reduced pressure to remove acetone to obtain a vegetable oil-based waterborne polyurethane coating.
[0044] Example 3
[0045] A preparation method of 1,5-diisocyanatopentane-polyurethane coating:
[0046] 100 parts of vegetable oil polyol FH-3170, 50 parts of 1,5-diisocyanatopentane, and 15 parts of flame retardant Pyrol99 were mixed in 30 parts of acetone, and 0.5 parts of imidazole type ionic liquid catalyst (anion is dicyanamide, cation is CB-5) was added, and the mixture was reacted at 50°C for 2h to obtain a prepolymer mixture;
[0047] Add 30 parts of a hydrophilic chain extender dihydroxy half ester (synthesized from glycerol and phthalic anhydride) to the prepolymer mixture, and react at 50° C. for 3 hours to obtain a polymer mixture;
[0048] The polymer mixture was cooled to 30°C and then 12 parts of a neutralizing agent, dimethylethanolamine, was added to neutralize the mixture to neutrality. 30 parts of deionized water were added to form a polyurethane emulsion by high-speed shear emulsification. The polyurethane emulsion was distilled under reduced pressure to remove acetone to obtain a vegetable oil-based waterborne polyurethane coating.
[0049] Example 4
[0050] A preparation method of 1,5-diisocyanatopentane-polyurethane coating:
[0051] 100 parts of vegetable oil polyol FHB-195, 53 parts of 1,5-diisocyanatopentane, and 15 parts of flame retardant Pyrol99 were mixed in 30 parts of acetone, and 0.5 parts of imidazole type ionic liquid catalyst (anion is dicyanamide, cation is CB-5) was added, and the mixture was reacted at 50°C for 2h to obtain a prepolymer mixture;
[0052] Add 30 parts of a hydrophilic chain extender dihydroxy half ester (synthesized from glycerol and phthalic anhydride) to the prepolymer mixture, and react at 50° C. for 3 hours to obtain a polymer mixture;
[0053] The polymer mixture was cooled to 30°C and then 12 parts of a neutralizing agent, dimethylethanolamine, was added to neutralize the mixture to neutrality. 30 parts of deionized water were added to form a polyurethane emulsion by high-speed shear emulsification. The polyurethane emulsion was distilled under reduced pressure to remove acetone to obtain a vegetable oil-based waterborne polyurethane coating.
[0054] Comparative Example 1
[0055] A method for preparing a vegetable oil-based waterborne polyurethane coating:
[0056] 100 parts of vegetable oil polyol FH-3170, 79 parts of MDI (diphenylmethane diisocyanate), and 15 parts of flame retardant Pyrol99 were mixed in 30 parts of acetone, and 0.5 parts of imidazole type ionic liquid catalyst (anion is dicyanamide, cation is CB-5) was added, and reacted at 50°C for 2h to obtain a prepolymer mixture;
[0057] Add 30 parts of a hydrophilic chain extender dihydroxy half ester (synthesized from glycerol and phthalic anhydride) to the prepolymer mixture, and react at 50° C. for 3 hours to obtain a polymer mixture;
[0058] The polymer mixture was cooled to 30°C and then 14 parts of a neutralizing agent triethylamine was added to neutralize it to neutrality. 30 parts of deionized water were added and emulsified at high speed to form a polyurethane emulsion. The polyurethane emulsion was distilled under reduced pressure to remove acetone to obtain a vegetable oil-based waterborne polyurethane coating.
[0059] Comparative Example 2
[0060] A method for preparing a vegetable oil-based waterborne polyurethane coating:
[0061] 100 parts of vegetable oil polyol FHB-195, 52 parts of 1,5-diisocyanatopentane, and 15 parts of flame retardant Pyrol99 were mixed in 30 parts of acetone, and 0.5 parts of imidazole type ionic liquid catalyst (anion is dicyanamide, cation is CB-5) was added, and the mixture was reacted at 50°C for 2h to obtain a prepolymer mixture;
[0062] Add 15 parts of dihydroxypropionic acid, a hydrophilic chain extender, to the prepolymer mixture, and react at 50° C. for 3 hours to obtain a polymer mixture;
[0063] The polymer mixture was cooled to 30°C and then 16 parts of a neutralizing agent triethylamine was added to neutralize it to neutrality. 30 parts of deionized water were added and emulsified at high speed to form a polyurethane emulsion. The polyurethane emulsion was distilled under reduced pressure to remove acetone to obtain a vegetable oil-based waterborne polyurethane coating.
[0064] Comparative Example 3
[0065] A method for preparing a vegetable oil-based waterborne polyurethane coating:
[0066] 100 parts of vegetable oil polyol FH-3170, 49 parts of 1,5-diisocyanatopentane, and 15 parts of flame retardant Pyrol99 were mixed in 30 parts of acetone, and 0.5 parts of imidazole type ionic liquid catalyst (anion is dicyanamide, cation is CB-5) was added, and the mixture was reacted at 50°C for 2h to obtain a prepolymer mixture;
[0067] Add 30 parts of a hydrophilic chain extender dihydroxy half ester (synthesized from glycerol and phthalic anhydride) to the prepolymer mixture, and react at 50° C. for 3 hours to obtain a polymer mixture;
[0068] The polymer mixture was cooled to 30°C and then 8 parts of a neutralizing agent triethylamine was added to neutralize it to neutrality. 30 parts of deionized water were added and emulsified at high speed to form a polyurethane emulsion. The polyurethane emulsion was distilled under reduced pressure to remove acetone to obtain a vegetable oil-based waterborne polyurethane coating.
[0069] Comparative Example 4
[0070] A method for preparing a vegetable oil-based waterborne polyurethane coating:
[0071] 100 parts of vegetable oil polyol FHB-195, 49 parts of 1,5-diisocyanatopentane, and 15 parts of flame retardant Pyrol99 were mixed in 30 parts of acetone, and 1 part of dibutyltin dilaurate was added, and the mixture was reacted at 50°C for 3 hours to obtain a prepolymer mixture;
[0072] Add 30 parts of a hydrophilic chain extender dihydroxy half ester (synthesized from glycerol and phthalic anhydride) to the prepolymer mixture, and react at 50° C. for 5 hours to obtain a polymer mixture;
[0073] The polymer mixture was cooled to 30°C and then 14 parts of a neutralizing agent triethylamine was added to neutralize it to neutrality. 30 parts of deionized water were added and emulsified at high speed to form a polyurethane emulsion. The polyurethane emulsion was distilled under reduced pressure to remove acetone to obtain a vegetable oil-based waterborne polyurethane coating.
[0074] Performance Testing
[0075] The bio-based polyurethane coatings prepared in Examples 1-4 and Comparative Examples 1-4 were subjected to performance characterization tests, and their drying time, pencil hardness, impact resistance, flexibility, and salt spray resistance were tested. The test data are shown in Table 1.
[0076] The coating was applied on a metal plate for testing, and the sample thickness was controlled to be approximately 240 μm.
[0077] The relevant determination methods for the prepared bio-based polyurethane coatings are as follows:
[0078] (1) Determine the actual drying time of the coating according to GB / T 1728-1979 (1989);
[0079] (2) Determine the pencil hardness of the coating according to GB / T 6739-2006;
[0080] (3) Determine the impact resistance of the coating according to GB / T 1732-1993;
[0081] (4) Determine the flexibility of the coating according to GB / T 1731-1993;
[0082] (5) The salt spray resistance of the coating was determined according to GB / T 1771-2007.
[0083] Table 1 Performance test results
[0084]
[0085] According to the data of the embodiments and comparative examples in Table 1, it can be seen that the bio-based polyurethane coating provided by the present invention has excellent mechanical properties and strong salt spray resistance. In combination with comparative example 1, the 1,5-diisocyanatopentane used in the present invention can achieve mechanical properties similar to those of MDI, and is environmentally friendly; in combination with comparative example 2, the use of a short-chain chain extender will reduce the mechanical properties of the material; in combination with comparative example 3, adding less neutralizer will cause the mechanical properties of the coating to decrease and the actual drying time to increase; in combination with comparative example 4, adding an ordinary catalyst will increase the reaction time and reduce the performance of the coating. Therefore, the appropriate proportion of isocyanate, hydrophilic chain extender, neutralizer, and ion catalyst are indispensable in the present invention.
[0086] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A 1,5-diisocyanatopentane-polyurethane coating, It is characterized in that The invention comprises the following raw materials in parts by weight: 100 parts of vegetable oil polyol, 40-75 parts of isocyanate, 30-40 parts of organic solvent, 0.1-2 parts of ionic liquid catalyst, 10-20 parts of flame retardant, 10-30 parts of hydrophilic chain extender, 10-30 parts of neutralizer and 20-40 parts of deionized water.
2. The 1,5-diisocyanate pentane-polyurethane coating according to claim 1, It is characterized in that The vegetable oil polyol is selected from at least one of olive oil polyol, peanut oil polyol, rapeseed oil polyol, cottonseed oil polyol, soybean oil polyol, coconut oil polyol, palm oil polyol, sesame oil polyol, corn oil polyol and sunflower oil polyol; the hydroxyl value of the vegetable oil polyol is 160-200 mgKOH / g.
3. The 1,5-diisocyanate pentane-polyurethane coating according to claim 1, It is characterized in that The isocyanate is 1,5-pentane diisocyanate; the organic solvent is selected from at least one of acetone, ethyl acetate, dichloromethane, dichloroethane, chloroform, n-hexane, tetrahydrofuran, and carbon tetrachloride.
4. The 1,5-diisocyanate pentane-polyurethane coating according to claim 1, It is characterized in that The ionic liquid catalyst is selected from at least one of a pyridine-type ionic liquid catalyst, an imidazole-type ionic liquid catalyst, and a long-chain fatty amine-type ionic liquid catalyst; the ionic liquid catalyst includes anions and cations.
5. The 1,5-diisocyanate pentane-polyurethane coating according to claim 4, It is characterized in that The anion is selected from at least one of dicyanamide, hexafluorophosphate, boron tetrafluoride, and bis(trifluoromethanesulfonyl)imide.
6. The 1,5-diisocyanate pentane-polyurethane coating according to claim 4, It is characterized in that The cation is selected from at least one of the following structural formulas CA-1, CA-2, CA-3, CA-4, CA-5, CA-6, CA-8, CA-9, CB-1, CB-2, CB-3, CB-4, CB-5, CB-6, CB-7, CB-8, CB-9, and CB-10, 7. The 1,5-diisocyanate pentane-polyurethane coating according to claim 1, It is characterized in that The flame retardant is selected from at least one of tributyl phosphate, tri(2-ethylhexyl) phosphate, tri(2-chloroethyl) phosphate, tri(2,3-dichloropropyl) phosphate, tri(2,3-dibromopropyl) phosphate, flame retardant Pyrol99, toluene-diphenyl phosphate, tricresyl phosphate, triphenyl phosphate, (2-ethylhexyl)-diphenyl phosphate, bis(4-hydroxyphenyl)phenylphosphine oxide, and casein; The neutralizing agent is selected from at least one of triethylamine, dimethylethanolamine and N,N-dimethylcyclohexylamine.
8. The 1,5-diisocyanate pentane-polyurethane coating according to claim 1, It is characterized in that The hydrophilic chain extender is a dihydroxy half ester; the dihydroxy half ester is prepared from a triol and a dibasic acid anhydride; wherein the triol is glycerol, and the dibasic acid anhydride is selected from at least one of phthalic anhydride, 1,2-cyclohexanedicarboxylic anhydride, nadic anhydride, and cyclopentane-1,2-dicarboxylic anhydride.
9. A method for preparing the 1,5-diisocyanate pentane-polyurethane coating according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1: mixing and reacting vegetable oil polyol, isocyanate, organic solvent, flame retardant and ionic liquid catalyst to obtain a prepolymer mixture; S2: adding a hydrophilic chain extender to the prepolymer mixture to react and obtain a polymer mixture; S3: After the polymer mixture is cooled, a neutralizing agent is added, and then deionized water is added to emulsify the mixture to form a polyurethane emulsion; S4: The polyurethane emulsion is obtained by removing the organic solvent through reduced pressure distillation.
10. The method for preparing the 1,5-diisocyanate pentane-polyurethane coating according to claim 8, It is characterized in that In S1, the mixed reaction temperature is 40-70°C, and the mixed reaction time is 1-3h; in S2, the reaction temperature is 40-70°C, and the reaction time is 2-5h; in S3, the temperature is lowered to 20-30°C.
Citation Information
Patent Citations
Modified bio-based waterborne polyurethane as well as preparation method and application thereof
CN117203258A
Vegetable oil polyol as well as preparation method and application thereof
CN117285694A
Vegetable oil polyol and preparation method of waterborne polyurethane coating
CN118290260A