High-sealing anti-curing silicon pu material
By introducing raw materials such as polyurethane and silicon rubber into silicon PU materials, a stable mesh structure and dynamic oxime urethane bond is formed, and a composite film layer is formed using aluminum foil to form, the problem of insufficient sealing and corrosion resistance of silicon PU materials is solved. It achieves efficient sealing and corrosion resistance, avoids curing of crusts, reduces additional treatment costs, and promotes its promotion in stadium floor materials.
Patent Information
- Application Number
- CN202411411696.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-08
AI Technical Summary
Existing silicon PU materials have poor sealing and corrosion resistance in stadium floor applications, resulting in the need of additional moisture-proof treatment, increasing costs and limiting their promotional use.
Adopt high-seal anti-curing silicon PU material formula, including polyurethane, silicone rubber, aluminum foil, silicone resin, thiol, methacryloyloxypropyltriethoxysilane, catalyst, polytetrahydrofuran ether glycol, chain extender and fillers, by forming a stable mesh structure and dynamic oxime urethane bond, improve acid and alkali resistance and sealing properties, and form a composite film layer structure through aluminum foil to avoid curing.
It significantly improves the corrosion resistance and sealing properties of silicon PU materials, avoids curing of crusts, reduces additional treatment costs, and is conducive to its wide application in stadium floor materials.
Smart Images

Figure CN118909532A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastic materials, in particular to a highly sealed and anti-curing silicon PU material. Background Art
[0002] Silicone PU material is a composite material of polyurethane and silicone rubber. As a new type of polymer material, silicon PU material combines the advantages of silicone and polyurethane. It has excellent weather resistance, elasticity, wear resistance, impact resistance and chemical stability. When used as the ground material of sports facilities, it has very good cushioning and ductility.
[0003] For example, CN115466505B involves a nano water-based silicone PU plastic material, including 13-150 parts of polyether polyol, 80-100 parts of paraffin, 3-5 parts of cross-linking agent, 0.5-1 part of dispersant, 220-300 parts of filler, 15-20 parts of additive, 0.3-0.5 part of color powder, 0.5-0.8 part of leveling agent, 20-25 parts of isocyanate, 1-2 parts of defoaming agent, 0.2-0.4 part of catalyst, and 20-25 parts of diluent.
[0004] The silicon PU material of the above patent solves the problem in the prior art that excessive inorganic fillers have poor dispersion in silicon PU plastic materials, which improves the high temperature resistance of the material while reducing the mechanical properties. However, it does not improve the poor sealing and corrosion resistance of the existing silicon PU materials. When the silicon PU material is used as the ground material of sports venues, an additional moisture-proof treatment process is still required to avoid the problem of ground damage caused by the crusting and curing of the silicon PU material. The high cost is not conducive to the promotion and use of silicon PU materials.
[0005] In order to improve the sealing and anti-corrosion performance of silicon PU materials, a highly sealing and anti-curing silicon PU material is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a highly sealed and curing-resistant silicon PU material to solve the problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides a highly sealed and anti-curing silicon PU material, comprising the following raw materials in the following mass proportions: Polyurethane 25-33%, silicone rubber 24-29%, aluminum foil 1-4%, leveling agent 1-3%, silicone resin 1-3%, mercaptan 1-2%, methacryloxypropyl triethoxysilane 1-3%, catalyst 1-2%, polytetramethylene glycol 1-2%, chain extender 1-2%, filler 1-3%, and the balance is water.
[0008] As a further improvement of the technical solution, the above-mentioned polyurethane, silicone rubber, polytetramethylene ether glycol, silicone resin, and thiol are mixed with water and put into a stirring tank and stirred for 1 hour. Then, a catalyst, aluminum foil, a leveling agent, a filler, and methacryloxypropyl triethoxysilane are added to the stirring tank and the temperature is raised to 100-120°C and reacted for 2 hours, and then the temperature is lowered to room temperature to obtain a silicon PU material.
[0009] As a further improvement of the present technical solution, the polyurethane is one of a polyester polyurethane or a polyurethaneamide polyurethane, the silicone rubber is a room temperature vulcanized silicone rubber, the chain extender includes dimethylglyoxime and isophorone diisocyanate, and the mass ratio of dimethylglyoxime to isophorone diisocyanate is 1:1.
[0010] As a further improvement of the technical solution, the thickness of the aluminum foil is in the range of 30-60 microns, and the mass proportion of the aluminum foil in the silicon PU material raw material is one of 1.8%, 2.4% or 3.1%.
[0011] As a further improvement of the technical solution, the leveling agent includes cellulose acetate butyrate and acrylic acid, and the mass ratio of cellulose acetate butyrate to acrylic acid is 2:1, and the thiol is a high molecular weight thiol.
[0012] As a further improvement of the present technical solution, the organic silicone resin is a phenyl hydrogenated silicone resin, and the mass proportion of the organic silicone resin in the silicon PU material raw material is one of 1.5%, 2.2%, 2.5% or 2.9%.
[0013] As a further improvement of the technical solution, the mass proportion of the polytetrahydrofuran ether diol in the silicon PU material raw material is one of 1.3%, 1.5% or 1.8%.
[0014] As a further improvement of the technical solution, the catalyst is stannous octoate.
[0015] As a further improvement of the technical solution, the waterproofing agent is one of acrylic resin or microcrystalline wax.
[0016] As a further improvement of the technical solution, the filler includes clay powder and coal slag, and the mass ratio of the clay powder to the coal slag is 1-3:1.
[0017] Compared with the prior art, the present invention has the following beneficial effects: In the high sealing and anti-curing silicon PU material, polyurethane, silicone rubber and other raw materials are used as the main materials for preparing the silicon PU material. Relying on the silicon-oxygen bonds with higher bond energy in the silicone resin molecules, a stable network structure is formed between the molecular chains of the silicon PU material, the movement of the molecular chains is restricted, and the acid and alkali resistance of the silicon PU material is improved, thereby improving the corrosion resistance of the silicon PU material. During the polymerization reaction, the hydroxyl group of polytetramethylene ether glycol reacts with the polyurethane to form an urethane bond, and then the connection effect of the chain extender helps to form a dynamic oxime urethane bond, and then the dynamic thermal reversibility of the dynamic oxime urethane bond is used to give the silicon PU material self-healing ability, thereby improving the tensile strength, elongation at break and toughness of the silicone rubber, and improving the sealing performance. In addition, materials such as aluminum foil in the silicon PU material can form a composite film layer structure, which effectively isolates the silicon PU material from contact with the air, thereby ensuring that the silicon PU material will not crust and solidify. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The tensile strength test of the present invention Figure 1 ; Figure 2 The tensile strength test of the present invention Figure 2 ; Figure 3 The tensile strength test of the present invention Figure 3 . DETAILED DESCRIPTION
[0019] The following will be combined with the accompanying drawings in the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1 The purpose of this embodiment is to provide a highly sealed and anti-curing silicon PU material, comprising the following raw materials in parts by weight: Polyurethane 25%, silicone rubber 29%, aluminum foil 1%, leveling agent 3%, silicone resin 1%, mercaptan 2%, methacryloxypropyl triethoxysilane 1%, catalyst 2%, polytetramethylene ether glycol 1%, chain extender 1%, waterproofing agent 2%, filler 3%, and the balance is water. The polyurethane, silicone rubber, polytetramethylene ether glycol, silicone resin, and mercaptan are mixed with water and put into a stirring tank and stirred for 1 hour. Then, the catalyst, aluminum foil, leveling agent, filler, and methacryloxypropyl triethoxysilane are added to the stirring tank and the temperature is raised to 100-120 ℃ for reaction for 2 hours, and then the temperature is cooled to room temperature to obtain the silicon PU material.
[0021] Among them, the polyurethane is one of polyester polyurethane or polyurethane amide polyurethane. Both types of polyurethane have good heat resistance and weather resistance, can improve the high temperature resistance of silicon PU materials, and can work stably for a long time in high temperature environment. The silicone rubber is room temperature vulcanized silicone rubber. Room temperature vulcanized silicone rubber has good softness. Even at extremely low temperatures, it still has good elasticity and softness, and is not easy to harden and crack. The chain extender includes dimethylglyoxime and isophorone diisocyanate, and the mass ratio of dimethylglyoxime to isophorone diisocyanate is 1:1. Dimethylglyoxime reacts with the isocyanate group in the polyurethane through its functional group to form an urethane bond, thereby increasing the molecular weight of the polyurethane, while isophorone diisocyanate reacts with the hydroxyl group at the end of the polymer molecule chain through its isocyanate group to form carbamate, thereby achieving chain extension of the polymer.
[0022] It is worth noting that the thickness of the aluminum foil ranges from 30 microns. In addition to having good flexibility and ductility, it also has good structural strength and corrosion resistance. The leveling agent includes cellulose acetate butyrate and acrylic acid, and the mass ratio of cellulose acetate butyrate to acrylic acid is 2:1. The role of the leveling agent is to improve the leveling of the silicon PU material, making its surface more uniform and smooth, and forming a more evenly distributed structural layer during the construction process. Thiol is a high molecular weight thiol, that is, the molecular structure usually contains one or more thiol groups, which can react with metal ions, metal oxides, acids, bases and other substances.
[0023] Furthermore, the organosilicon resin is a phenyl hydrogenated silicone resin, and the catalyst is stannous octoate, which can promote the reaction of the resin and shorten the drying and curing time of the silicon PU material. The filler includes clay powder and coal slag, and the mass ratio of clay powder to coal slag is 3:1.
[0024] Example 2 The purpose of this embodiment is to provide a highly sealed and anti-curing silicon PU material, comprising the following raw materials in parts by weight: Polyurethane 29%, silicone rubber 26%, aluminum foil 2%, leveling agent 2%, silicone resin 2.3%, mercaptan 1.6%, methacryloxypropyl triethoxysilane 2%, catalyst 1.5%, polytetramethylene ether glycol 1.8%, chain extender 1.5%, waterproofing agent 1.2%, filler 2.1%, and the balance is water. The polyurethane, silicone rubber, polytetramethylene ether glycol, silicone resin, and mercaptan are mixed with water and put into a stirring tank and stirred for 1 hour. Then, the catalyst, aluminum foil, leveling agent, filler, and methacryloxypropyl triethoxysilane are added to the stirring tank and the temperature is raised to 100-120 ° C for reaction for 2 hours, and then the temperature is cooled to room temperature to obtain the silicon PU material.
[0025] Wherein, the polyurethane is one of polyester polyurethane or polyurethaneamide polyurethane, and the silicone rubber is room temperature vulcanized silicone rubber; The chain extender includes dimethylglyoxime and isophorone diisocyanate, and the mass ratio of dimethylglyoxime to isophorone diisocyanate is 1:1.
[0026] It is worth noting that the thickness of the aluminum foil ranges from 50 μm, the leveling agent includes cellulose acetate butyrate and acrylic acid, and the mass ratio of cellulose acetate butyrate to acrylic acid is 2:1, and the thiol is a high molecular weight thiol.
[0027] Furthermore, the organosilicon resin is a phenyl hydrogenated silicone resin, the catalyst is stannous octoate, the filler includes clay powder and coal slag, and the mass ratio of the clay powder to the coal slag is 2:1.
[0028] Example 3 The purpose of this embodiment is to provide a highly sealed and anti-curing silicon PU material, comprising the following raw materials in parts by weight: Polyurethane 33%, silicone rubber 24%, aluminum foil 4%, leveling agent 1%, silicone resin 3%, mercaptan 1%, methacryloxypropyl triethoxysilane 3%, catalyst 1%, polytetramethylene ether glycol 2%, chain extender 2%, waterproofing agent 1%, filler 1%, and the balance is water. The polyurethane, silicone rubber, polytetramethylene ether glycol, silicone resin, and mercaptan are mixed with water and put into a stirring tank and stirred for 1 hour. Then, the catalyst, aluminum foil, leveling agent, filler, and methacryloxypropyl triethoxysilane are added to the stirring tank and the temperature is raised to 100-120 ℃ for reaction for 2 hours, and then the temperature is cooled to room temperature to obtain the silicon PU material.
[0029] Wherein, the polyurethane is one of polyester polyurethane or polyurethaneamide polyurethane, and the silicone rubber is room temperature vulcanized silicone rubber; The chain extender includes dimethylglyoxime and isophorone diisocyanate, and the mass ratio of dimethylglyoxime to isophorone diisocyanate is 1:1.
[0030] It is worth noting that the thickness of the aluminum foil ranges from 60 μm, the leveling agent includes cellulose acetate butyrate and acrylic acid, and the mass ratio of cellulose acetate butyrate to acrylic acid is 2:1, and the thiol is a high molecular weight thiol.
[0031] Furthermore, the organosilicon resin is a phenyl hydrogenated silicone resin, the catalyst is stannous octoate, the filler includes clay powder and coal slag, and the mass ratio of the clay powder to the coal slag is 1:1.
[0032] The water resistance of the silicon PU materials prepared in Examples 1-3 was tested. The prepared silicon PU materials were brushed on cement blocks for multiple times, and the film thickness was controlled at 1.2-1.5 mm. They were immersed in 1% alkaline water for 7 days, and the stratification phenomenon of the materials was observed and the results were recorded in Table 1.
[0033] Table 1 Water resistance test results of silicon PU materials prepared in Examples 1-3 It can be seen from Table 1 that the silicon PU materials prepared in Examples 1-3 have no delamination and hollowing phenomenon, indicating that the prepared silicon PU materials have good sealing and anti-corrosion properties.
[0034] In the present invention, polyurethane with good heat resistance and weather resistance and flexible room temperature vulcanized silicone rubber with good elasticity are selected as the main materials for preparing the silicon PU material, dimethylglyoxime and isophorone diisocyanate are used as chain extenders, and organic silicone resin is used as an anti-corrosion modifier for coordination, and the silicon-oxygen bonds with higher bond energy in the organic silicone resin molecules are relied on to form a stable network structure between the molecular chains of the silicon PU material, restrict the movement of the molecular chains, improve the acid and alkali resistance of the silicon PU material, and thus improve the corrosion resistance of the silicon PU material, and then polytetrahydrofuran ether diol is used as a cross-linking agent, and the self-healing ability of the silicon PU material is given through the dynamic oxime urethane bond, the tensile strength, elongation at break and toughness of the silicone rubber are improved, and the sealing performance is improved, and the aluminum foil in the silicon PU material can form a composite film layer structure, effectively isolating the silicon PU material from contact with the air, and avoiding reaction with trace moisture in the air, thereby ensuring that the silicon PU material will not be crusted and solidified.
[0035] Example 4 During the production process of silicon pu materials, the heating reaction temperature in the stirring tank will affect the reaction rate of the polyurethane system and the catalytic efficiency of the catalyst. Too low a temperature will lead to low catalyst activity, a slow reaction rate of the polyurethane system, and easy production of by-products that affect the quality of the silicon pu materials produced. Too high a temperature will cause excessive polymerization, resulting in excessive cross-linking of the product, affecting the physical and chemical properties of the silicon pu materials produced.
[0036] Therefore, in order to verify the influence of reaction temperature on the performance of the produced silicon PU material, on the basis of Example 2, the heating reaction temperature of the stirring kettle during the preparation of the silicon PU material was set to 90 ℃, 100 ℃, 110 ℃, 120 ℃, and 140 ℃, and then the tensile strength of the prepared silicon PU material was tested according to "GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber". The test results are shown in Table 2.
[0037] Table 2 Comparison of tensile strength of silicon PU materials prepared at different heating reaction temperatures According to Table 2, when the stirring kettle heating reaction temperature is 90 ℃ and 140 ℃, the tensile strength of the silicon pu material prepared is significantly lower than that of the silicon pu material prepared at 100 ℃, 110 ℃ and 120 ℃, that is, when the stirring kettle heating reaction temperature is lower than 100 ℃ or higher than 120 ℃, the performance of the prepared silicon pu material will decrease, and too low or too high reaction temperature will have a negative impact on the performance of the output silicon pu material.
[0038] Example 5 In the present invention, stannous octoate is preferably used as a catalyst. Stannous octoate can catalyze the cross-linking reaction of polyurethane and silicone rubber, so that the linear silicone rubber molecular chain forms a three-dimensional network structure through the cross-linking points, thereby accelerating the generation of silicon PU materials. In addition, stannous octoate has good compatibility with aluminum foil, silicone resin, mercaptan, methacryloxypropyl triethoxysilane, polytetramethylene glycol, etc., and can effectively promote polymerization reactions and improve the performance of silicon PU materials.
[0039] Stannous octoate is an organic metal compound containing tin (II) ions and octanoic acid coordination ligands. It accelerates the cross-linking reaction of polymers by interacting with functional groups in the reactants (such as hydroxyl, silyl, isocyanate, etc.). Its mechanism of action is mainly reflected in: Reaction of isocyanate with hydroxyl groups: During the formation of polyurethane, isocyanate (–NCO) reacts with polyol (–OH) to form a carbamate (–NHCOO–) structure. This reaction can be catalyzed by stannous octoate to accelerate the reaction rate: Stannous octoate enhances the nucleophilic activity of isocyanate through the affinity of the nucleophilic center of the tin atom with the isocyanate group, making the reaction easier to occur; In the cross-linking reaction of polyurethane and silicone rubber, stannous octoate accelerates the cross-linking of polyols, isocyanates and silicone rubber. Through the action of tin catalyst, the isocyanate group (–NCO) of polyurethane reacts with the silanol group (–Si–OH) or hydroxyl group (–OH) in silicone rubber to form a network with Si–O–Si and urethane structure, thereby constructing silicon PU material. The chemical formula of the cross-linking reaction can be simplified as: This allows linear molecules to connect through cross-linking points, forming a more stable three-dimensional network structure.
[0040] In order to determine the influence of the mass proportion of the catalyst, i.e., stannous octoate, on the performance of the prepared silicon PU material, based on Example 2, only the mass proportion of stannous octoate in the silicon PU material raw material was set to 0.5%, 1.0%, 1.5%, 2.0%, and 2.5%, and the silicon PU material was prepared. Then, the tensile strength of the prepared silicon PU material was tested according to GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber. The test results are as follows: Figure 1 shown.
[0041] according to Figure 1 It can be seen that under the working conditions of this embodiment, the tensile strength of the silicon PU material prepared when the mass proportion of stannous octoate is 0.5% or 2.5% is significantly lower than the tensile strength when the mass proportion of stannous octoate is 1.0%, 1.5% or 2.0%, that is, when the mass proportion of stannous octoate is 1-2%, the prepared silicon PU material has good tensile resistance.
[0042] Example 6 Silicone resin is a thermosetting polysiloxane polymer with a highly cross-linked structure. It has the dual characteristics of organic resin and inorganic material and has unique physical and chemical properties. The silicone resin in silicon PU material can form a stable protective film and achieve an anti-corrosion effect through the oxidation of unsaturated fat functional groups in the resin and polyaddition reaction.
[0043] First, in order to verify that the silicone resin is one of the important components for improving the anti-corrosion performance of the silicon PU material, on the basis of Example 2, only the silicone resin is missing or only the silicone resin is replaced by epoxy resin to prepare the silicon PU material, and then the water resistance of the silicon PU material is tested. The prepared silicon PU material is brushed on the cement block several times, and the film thickness is controlled at 1.2-1.5 mm. It is immersed in 1% alkaline water for 7 days, and the stratification phenomenon of the material is observed and the results are recorded in Table 3.
[0044] Table 3 Water resistance test results of silicon PU materials It can be seen from Table 2 that based on Example 2, when the silicone resin is missing or the silicone resin is replaced by epoxy resin, the prepared silicon PU material will show delamination and hollowing phenomenon in the water resistance test. Therefore, it can be shown that silicone resin is one of the important components to improve the anti-corrosion performance of silicon PU materials.
[0045] Secondly, the silicon-oxygen bond energy of the silicone resin is relatively high. By modifying it with other materials, the tensile strength of the material can be further improved. The silicone resin includes methyl silicone resin, phenyl hydrogen silicone resin, phenolic silicone resin, etc. In order to determine the influence of the composition and mass proportion of the silicone resin on the tensile strength of the silicon PU material, on the basis of Example 2, the silicone resins are respectively set to methyl silicone resin, phenyl hydrogen silicone resin, and phenolic silicone resin, and the mass proportions of the silicone resin in the silicon PU material raw material are respectively set to 0.8%, 1.5%, 2.2%, 2.5%, 2.9%, and 3.2%. The silicon PU material is prepared, and the tensile strength of the silicon PU material is tested according to GB / T 528-2009 Determination of Tensile Stress-Strain Properties of Vulcanized Rubber or Thermoplastic Rubber. The test results are as follows: Figure 2 shown.
[0046] according to Figure 2 It can be seen that under the working conditions of this embodiment, when the mass proportion of the organic silicone resin is 0.8% or 3.2%, that is, when the mass proportion of the organic silicone resin is not 1-3%, the tensile strength of the silicon PU material is significantly reduced; When the silicone resin is one of methyl silicone resin, phenyl hydrogen silicone resin or phenolic silicone resin, and the mass proportion of the silicone resin is 1.5%, 2.2%, 2.5% or 2.9%, the silicon PU material has good tensile strength, and when the silicone resin is phenyl hydrogen silicone resin and the mass proportion is 2.2%, the silicon PU material has a higher tensile strength.
[0047] Example 7 When improving the sealing performance of silicon pu materials, polytetramethylene glycol is added to cooperate with polyurethane, silicone rubber, chain extender and other raw materials. During the polymerization reaction, the hydroxyl group of polytetramethylene glycol reacts with polyurethane to form an urethane bond, and then the dynamic oxime urethane bond is formed through the connecting effect of the chain extender. The dynamic thermal reversibility of the dynamic oxime urethane bond is then used to give the silicon pu material self-healing ability. This self-healing ability helps to repair scratches or splicing interfaces, further improve the sealing performance, and further improve the tensile strength, elongation at break and toughness of the silicon pu material. By adjusting the mass proportion of polytetramethylene glycol, the hard segment phase content and the strain-induced crystallization of the soft segment of the silicon pu material can be regulated, thereby achieving simultaneous enhancement and toughening, and achieving the purpose of improving the sealing performance of the silicon pu material.
[0048] Polytetramethylene glycol is a linear polyol with a hydroxyl (–OH) terminal. During the reaction, the hydroxyl group in PTHF reacts with the isocyanate group (–NCO) in the material to form an urethane bond (–NHCOO–). This reaction is called an addition reaction or polymerization reaction, and its reaction formula is: Among them, R represents the isocyanate group in the material, and R' represents the organic group in polytetramethylene ether diol. The main purpose of this reaction is to form an urethane bond to combine polytetramethylene ether diol with the polyurethane chain to enhance the elasticity, toughness and sealing performance of the material.
[0049] In the chain extender, dimethylglyoxime is a compound with an oxime group (–C=NOH), which can help extend the polymer chain in the polymerization reaction. The isocyanate group of isophorone diisocyanate reacts with the hydroxyl group in polytetramethylene ether diol to form an urethane bond. At the same time, the amino group in dimethylglyoxime reacts with the isocyanate group to form an oxime urethane bond (–C=NO–). This oxime urethane bond has dynamic reversibility and can dissociate when the temperature rises and re-form after cooling. This property enables the material to repair its scratches or interface damage by heating. The reaction mechanism is: Among them, R is the organic part of the polyurethane, and R' is the oxime part. Through this process, the chain extender can effectively extend the polymer chain and form a dynamically reversible oxime urethane bond.
[0050] In order to determine that polytetramethylene ether glycol is one of the important components for improving the sealing performance of silicon PU materials, and that 1-2% by mass of polytetramethylene ether glycol is one of the important factors for improving the sealing performance of silicon PU materials, on the basis of Example 2, only polytetramethylene ether glycol is removed, or the mass proportion of polytetramethylene ether glycol is set to 0.5%, 1.3%, 1.5%, 1.8%, 2.3%, and silicon PU materials are prepared. According to GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber, the tensile strength of the silicon PU material is tested. The test results are as follows: Figure 3 shown.
[0051] according to Figure 3 It can be known that under the working conditions of this embodiment, when polytetramethylene ether glycol is removed (i.e., the mass proportion of polytetramethylene ether glycol is 0), or the mass proportion of polytetramethylene ether glycol is 0.5%, 2.3%, that is, the mass proportion of polytetramethylene ether glycol is not 1-2%, the tensile strength of the silicon pu material is significantly lower than the tensile strength of the silicon pu material when the mass proportion of polytetramethylene ether glycol is 1.3%, 1.5%, 1.8%. Therefore, it can be explained that polytetramethylene ether glycol is one of the important components for improving the sealing performance of silicon pu materials, and the 1-2% mass proportion of polytetramethylene ether glycol is one of the important factors for improving the sealing performance of silicon pu materials.
[0052] Example 8 The aluminum foil material itself has good air barrier properties and corrosion resistance. During the preparation of silicon pu materials, the aluminum foil material is compounded with other materials to form an aluminum foil composite film, which isolates the silicon pu material from the air, preventing the silicon pu material from contacting with moisture in the air, thereby preventing the silicon pu material from crusting and solidifying.
[0053] First, during the preparation of silicon pu materials, small-particle aluminum foil materials are pushed and moved in the fluid due to the shear force and pressure gradient force exerted by the fluid on the aluminum foil. During the movement of the aluminum foil materials, the aluminum foil materials will be brought together to form initial contact and stacking; When aluminum foil materials come into contact with each other in a fluid, the van der Waals force or electrostatic attraction caused by the electric charge on the surface of the aluminum foil materials will cause adsorption and bonding between the aluminum foil materials. As time goes by, the stacked aluminum foil materials increase, and the interaction between the aluminum foil materials will gradually increase. Under the combined effect of fluid dynamics and the interaction of the aluminum foil materials, the aluminum foil materials will gradually converge and tightly combine together, combining with polyurethane, silicone rubber and other materials to form a continuous aluminum foil composite film, which can isolate the air and prevent the silicone PU material from absorbing water and forming a crust and solidifying.
[0054] In order to determine that aluminum foil is one of the important components to prevent silicon pu material from crusting and solidifying, and that 1-4% by mass of aluminum foil is one of the important factors to prevent silicon pu material from crusting and solidifying, on the basis of Example 2, only the aluminum foil is removed, or the mass proportion of aluminum foil in the silicon pu material raw material is set to 0.8%, 1.8%, 2.4%, 3.1%, 4.5%, and silicon pu material is prepared. The silicon pu material is applied on the cement block several times, and the film thickness is controlled to be 1.2-1.5 mm. The film is immersed in 1% alkaline water for 7 days, and the stratification phenomenon of the material is observed. The test results are included in Table 4.
[0055] Table 4 Water resistance test results of silicon PU materials It can be seen from Table 3 that under the working conditions of this embodiment, when the aluminum foil is removed (i.e., the mass proportion of the aluminum foil is 0), or the mass proportion of the aluminum foil is 0.8%, 4.5%, that is, the mass proportion of the aluminum foil is not 1-4%, the prepared silicon pu material will show stratification and hollowing phenomenon in the water resistance test, and when the mass proportion of the aluminum foil is 1.8%, 2.4%, and 3.1%, the prepared silicon pu material will not show stratification and hollowing phenomenon in the water resistance test. Therefore, it can be explained that aluminum foil is one of the important components to prevent the silicon pu material from crusting and solidifying, and the 1-4% mass proportion of aluminum foil is one of the important factors to prevent the silicon pu material from crusting and solidifying.
[0056] In addition, during the preparation of silicon pu materials, a waterproof film can be formed on the surface of the material by adding a waterproof agent, which cooperates with the aluminum foil composite film to prevent water penetration and enhance the waterproof ability of the silicon pu material. The waterproof agent has various components. In this embodiment, acrylate resin or microcrystalline wax is preferably used. Among them, acrylate resin can fill tiny holes on the surface of an object and play a sealing role. The chemical composition of acrylate resin makes its surface tension smaller than the surface tension of water, so that water cannot form droplets on its surface, thereby effectively preventing water penetration; microcrystalline wax can form a uniform wax film on the surface of the silicon pu material to isolate external water vapor and achieve the purpose of protecting the rubber.
[0057] In order to determine that the waterproofing agent is one of the important components that affect the prevention of crusting and curing of silicon PU materials, on the basis of Example 2, only the waterproofing agent is removed, or the waterproofing agent component is set to acrylic resin or microcrystalline wax, and the silicon PU material is prepared. The silicon PU material is applied to the cement block several times, and the film thickness is controlled to be 1.2-1.5 mm. It is soaked in 1% alkaline water for 7 days, and the stratification phenomenon of the material is observed. The test results are recorded in Table 5.
[0058] Table 5 Water resistance test results of silicon PU materials According to Table 5, under the working conditions of this embodiment, when the waterproofing agent is removed from the ingredients, the prepared silicon pu material will have obvious hollowing phenomenon in the water resistance test, which shows that the waterproofing agent is one of the important components that affect the crusting and curing of the silicon pu material, and when the waterproofing agent is acrylate resin or microcrystalline wax, the prepared silicon pu material will not have stratification and hollowing phenomenon in the water resistance test, indicating that using acrylate resin or microcrystalline wax as a waterproofing agent can achieve a good waterproof effect.
[0059] Example 9 According to the method provided in the above embodiment and the determined optimal preparation parameters, the silicon PU material was prepared, and then the water resistance test was carried out. The silicon PU material was brushed on the cement block several times, and the film thickness was controlled at 1.2-1.5 mm. It was soaked in 1% alkaline water for 7 days, and the stratification phenomenon of the material was observed; Tests have shown that under the working conditions of this embodiment, the silicon PU material will not show stratification and hollowing phenomena, and the sealing and corrosion resistance of the silicon PU material are improved. When the silicon PU material is used as the ground material of a sports venue, it is no longer necessary to apply an additional moisture-proof treatment process, which can reduce costs and is conducive to the promotion and use of silicon PU materials.
[0060] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A highly sealed and anti-curing silicon PU material, characterized in that: Including the following raw materials by mass: Polyurethane 25-33%, silicone rubber 24-29%, aluminum foil 1-4%, leveling agent 1-3%, silicone resin 1-3%, mercaptan 1-2%, methacryloxypropyl triethoxysilane 1-3%, catalyst 1-2%, polytetramethylene glycol 1-2%, chain extender 1-2%, waterproofing agent 1-2%, filler 1-3%, and the balance is water.
2. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: Polyurethane, silicone rubber, polytetramethylene glycol, silicone resin, and mercaptan are mixed with water and put into a stirring kettle and stirred for 1 hour. Then, a catalyst, aluminum foil, a leveling agent, a filler, and methacryloxypropyltriethoxysilane are added to the stirring kettle and the temperature is raised to 100-120 ° C and reacted for 2 hours. Then, the temperature is cooled to room temperature and the silicon PU material is obtained.
3. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: The polyurethane is one of polyester polyurethane or polyurethane amide polyurethane, the silicone rubber is room temperature vulcanized silicone rubber, the chain extender includes dimethylglyoxime and isophorone diisocyanate, and the mass ratio of dimethylglyoxime to isophorone diisocyanate is 1:
1.
4. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: The thickness of the aluminum foil is in the range of 30-60 microns, and the mass proportion of the aluminum foil in the silicon PU material raw material is one of 1.8%, 2.4% or 3.1%.
5. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: The leveling agent comprises cellulose acetate butyrate and acrylic acid, and the mass ratio of cellulose acetate butyrate to acrylic acid is 2:
1. The thiol is a high molecular weight thiol.
6. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: The organic silicone resin is a phenyl hydrogenated silicone resin, and the mass proportion of the organic silicone resin in the silicon PU material raw material is one of 1.5%, 2.2%, 2.5% or 2.9%.
7. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: The mass proportion of the polytetramethylene ether diol in the silicon PU material raw material is one of 1.3%, 1.5% or 1.8%.
8. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: The catalyst is stannous octoate.
9. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: The waterproofing agent is one of acrylic resin or microcrystalline wax.
10. The high sealing and curing resistant silicon PU material according to claim 1, characterized in that: The filler includes clay powder and coal slag, and the mass ratio of the clay powder to the coal slag is 1-3:1.
Citation Information
Patent Citations
A silicon PU plastic material
CN115466505B