Ultralow-viscosity water-based pressure-sensitive adhesive for polaroid as well as preparation method and application of ultralow-viscosity water-based pressure-sensitive adhesive
By using ultra-low viscosity water-sensitive pressure-sensitive adhesive in the polyacrylate protective film, combining polymer amphiphilic emulsifier and highly reactive epoxy crosslinking agent, the problem of excessive tearing of the polyacrylate protective film is solved. Reduce costs and improve market competitiveness.
Patent Information
- Application Number
- CN202411172702.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
AI Technical Summary
After the polyacrylate protective film is pasted with a polarizer through a conventional polyacrylate glue layer, the surface resistance of the glue layer is large, resulting in too high tearing film voltage and easy breakdown of the touch sensor, increasing costs and reducing market competitiveness.
An ultra-low viscosity water-sensitive pressure-sensitive adhesive for polarizer is used, which includes a resin composition and a curing agent. The mass ratio of the resin composition to the curing agent is 100:3-5, and a polymer amphiphilic emulsifier and high activity are used. Epoxy crosslinking agent reduces the surface resistance of the glue layer through crosslinking reaction and reduces the tearing voltage of the film.
Achieve lower polarity and surface energy, improve wetting and exhaust properties, reduce film tearing pressure, avoid touch sensor breakdown, significantly reduce the cost of polyacrylate protective film, and improve market competitiveness .
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic synthesis, and in particular to an ultra-low viscosity water-based pressure-sensitive adhesive for a polarizer, and a preparation method and application thereof. Background Art
[0002] In recent years, with the development of various electronic products such as smart phones and tablets, in order to prevent the screens of electronic products from being scratched or worn during processing and transportation, a protective film is generally attached to the surface of the polarizer of the screen. Among various types of protective films, polyacrylate protective film is a functional protective film made of transparent polyester film as the base material, single-sided coating of polyacrylate glue, and then attached with a release film. Polyacrylate protective film has the advantages of smooth surface, good adsorption performance, and low cost. It is mainly used for shipment protection of polarizers.
[0003] There is a touch module behind the TP glass of the display screen. If the tearing voltage is too high, it will break through the touch sensor and cause damage. Therefore, major screen manufacturers have set certain requirements for the tearing voltage, which is generally less than 400V. After the polyacrylate protective film is attached to the polarizer through the conventional polyacrylate glue layer, the tearing voltage is too high and it is easy to break through the touch sensor. In order to reduce the tearing voltage of the polyacrylate protective film, antistatic agents are usually added to the polyacrylate glue, which undoubtedly increases the cost of the polyacrylate protective film and reduces its market competitiveness. Summary of the invention
[0004] The problem in the prior art is that after the polyacrylate protective film is attached to the polarizer through a conventional polyacrylate glue layer, the surface resistance of the glue layer is large, the tearing voltage is too high, and the touch sensor is easily broken down. In view of the above problems, the present invention provides an ultra-low viscosity water-based pressure-sensitive adhesive for a polarizer, which includes a resin composition and a curing agent, wherein the mass ratio of the resin composition to the curing agent is 100:3-5;
[0005] The resin composition, in parts by weight, comprises the following raw materials:
[0006]
[0007]
[0008] The polymer amphiphilic emulsifier is a β-carboxyethyl acrylate-o-phenylphenoxyethyl acrylate amphiphilic block polymer, and the preparation method of the polymer amphiphilic emulsifier comprises the following steps:
[0009] Under nitrogen protection, 60g of β-carboxyethyl acrylate, 80g of ethanol, 2g of 2-cyano-2-propylbenzodisulfide, and 0.8g of azobisisobutyronitrile are added to a reactor, and stirred at a constant temperature of 60°C for reaction for 12-24h, and then 20g of o-phenylphenoxyethyl acrylate and 2.2g of azobisisobutyronitrile are added to the reaction system, and stirred at a constant temperature of 60°C for reaction for 12-24h, and then AMP-95 is added to the reaction system for neutralization reaction, so that the pH of the reaction system is 7, and finally the solvent is removed by vacuum at 65°C to obtain β-hydroxyethyl acrylate-tert-butyl methacrylate amphiphilic block polymer, that is, a polymer amphiphilic emulsifier;
[0010] The highly active epoxy crosslinking agent contains 8 epoxy groups in its molecular structure.
[0011] Preferably, the preparation method of the highly active epoxy crosslinking agent comprises the following steps:
[0012] (1) 1,2,4,5-benzenetetraamine and excess epichlorohydrin are added to anhydrous ethanol, and the mixture is stirred at a constant temperature of 30-50° C. The reaction is monitored by FTIR. When the absorption peak of the amino group disappears in the infrared spectrum, the reaction is completed. After the reaction is completed, the excess epichlorohydrin is removed by vacuum distillation to obtain an intermediate product I. The chemical structure of the intermediate product I is as follows:
[0013]
[0014] (2) Then, alkali is added dropwise to the above reaction system while stirring, and the reaction is stirred at a constant temperature of 35-70° C., and the progress of the reaction is monitored by FTIR. When the absorption peak of the epoxy group in the infrared spectrum no longer increases, the addition of alkali is stopped, and the reaction is terminated. Then, methyl isobutyl ketone and deionized water are added to the reaction system of step (2), and after stirring evenly, liquid separation and extraction are performed, and the water layer is removed. The remaining extract is placed at a constant temperature of 50-65° C. and stirred for 1-3 hours. Then, the reaction solution is washed with sodium chloride aqueous solution until it is neutral, and the solvent is removed by reduced pressure distillation to obtain a high-activity epoxy-type crosslinking agent. The chemical structure of the high-activity epoxy-type crosslinking agent is as follows:
[0015]
[0016] Preferably, the alkali in step (2) is an aqueous NaOH solution or an aqueous KOH solution with a mass concentration of 15-40%.
[0017] Preferably, the mass concentration of the sodium chloride aqueous solution is 2-8%.
[0018] Preferably, the cross-linking monomer includes at least one of tripropylene glycol diacrylate, trimethylolpropane triacrylate, and 1,6-hexanediol diacrylate.
[0019] Preferably, the curing agent is an organosilicon crosslinking agent Silicone-9301, purchased from Beijing Baiyuan Chemical Co., Ltd.
[0020] Preferably, the initiator comprises potassium persulfate or ammonium persulfate.
[0021] Preferably, the reducing agent is a sodium sulfinate derivative, specifically Bruggolite FF6M.
[0022] Preferably, the preparation method of the ultra-low viscosity water-based pressure-sensitive adhesive for polarizer comprises the following steps:
[0023] (1) After fully mixing a highly active epoxy crosslinking agent, butyl acrylate, styrene, acrylic acid, and a crosslinking monomer according to the formula amount, the mixture is then mixed with 13 / 25 of the formula amount of deionized water, butadiene, 3 / 5 of the formula amount of an initiator, n-dodecyl mercaptan, and a polymer amphiphilic emulsifier, and the mixture is stirred at high speed and emulsified under pressure to obtain a monomer pre-emulsion;
[0024] (2) heating the remaining amount of deionized water to 80° C., adding 5-8% of the total mass of the monomer pre-emulsion obtained in step (1) and the remaining initiator, stirring and reacting at a constant temperature of 0.3-1 MPa for 20 min, then dropping the remaining amount of monomer pre-emulsion within 3-5 h, stirring at a constant temperature for 1 h, then reducing the temperature of the reaction system to 60-65° C., and starting to drop the reduced agent into the reaction system while stirring, the dropping time is controlled within 30-45 min. After the dropwise addition is completed, stirring and reacting at a constant temperature for 1 h, then reducing the temperature of the reaction system to below 25° C., adding the pH adjuster in the formula amount so that the pH of the reaction system is 7-8, stirring evenly, filtering and discharging the material, and obtaining an ultra-low viscosity water-based pressure-sensitive adhesive for polarizer.
[0025] Preferably, the pH adjuster is aqueous ammonia with a mass concentration of 25-28%.
[0026] The present invention has the following beneficial effects:
[0027] (1) The ultra-low viscosity water-based pressure-sensitive adhesive for polarizer obtained by the present invention belongs to a styrene-butadiene emulsion type pressure-sensitive adhesive. Compared with an acrylic ester emulsion type pressure-sensitive adhesive, it has lower polarity, lower surface energy after film formation, better wettability and air discharge, better bonding performance, lower peeling force between the protected substrate and the film tearing pressure, and is not easy to break through the touch sensor in the touch mold on the rear side of the display screen TP glass;
[0028] (2) The present invention uses a self-made ultra-low viscosity water-based pressure-sensitive adhesive as the adhesive layer of the polyacrylate protective film, and no antistatic agent of any type is added to the pressure-sensitive adhesive, which significantly reduces the cost of the polyacrylate protective film and improves market competitiveness;
[0029] (3) The present invention uses a self-made high molecular amphiphilic emulsifier, namely, β-carboxyethyl acrylate-o-phenylphenoxyethyl acrylate amphiphilic block polymer, as an emulsifier in the preparation process of the ultra-low viscosity water-based pressure-sensitive adhesive. The obtained emulsifier molecular structure contains abundant benzene ring structures and has better compatibility with the styrene-butadiene rubber molecular chain in the pressure-sensitive adhesive material system, and there is a stronger intermolecular force between the two. The obtained styrene-butadiene emulsion type pressure-sensitive adhesive has better dispersibility and stability, the pressure-sensitive adhesive is more evenly distributed on the surface of the polyester substrate, the surface resistance of the adhesive layer is smaller, and the film tearing voltage is also smaller;
[0030] (4) At room temperature, the epoxy group of the highly active epoxy crosslinking agent obtained by the present invention undergoes a crosslinking reaction with the carboxyl group on the styrene-butadiene rubber molecular chain in the pressure-sensitive adhesive latex system, further increasing the crosslinking density of the pressure-sensitive adhesive layer. At the same time, the carboxyl group on the styrene-butadiene rubber molecular chain reacts with the epoxy group of the highly active epoxy crosslinking agent to generate hydroxy esters. The hydroxyl group is hydrophilic, which is beneficial to reducing the volume resistance and surface resistance of the pressure-sensitive adhesive. The obtained pressure-sensitive adhesive layer has a better antistatic effect, and the film tearing voltage is further reduced. DETAILED DESCRIPTION
[0031] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0032] The highly active epoxy crosslinking agent in the following embodiments of the present invention is prepared as follows:
[0033] (1) 1,2,4,5-benzenetetraamine and excess epichlorohydrin are added to anhydrous ethanol, and the mixture is stirred at a constant temperature of 30-50° C. The reaction is monitored by FTIR. When the absorption peak of the amino group disappears in the infrared spectrum, the reaction is completed. After the reaction is completed, the excess epichlorohydrin is removed by vacuum distillation to obtain an intermediate product I. The chemical structure of the intermediate product I is as follows:
[0034]
[0035] (2) Then, alkali is added dropwise to the above reaction system while stirring, and the reaction is stirred at a constant temperature of 35-70° C., and the progress of the reaction is monitored by FTIR. When the absorption peak of the epoxy group in the infrared spectrum no longer increases, the addition of alkali is stopped, and the reaction is terminated. Then, methyl isobutyl ketone and deionized water are added to the reaction system of step (2), and after stirring evenly, liquid separation and extraction are performed, and the water layer is removed. The remaining extract is placed at a constant temperature of 50-65° C. and stirred for 1-3 hours. Then, the reaction solution is washed with sodium chloride aqueous solution until it is neutral, and the solvent is removed by reduced pressure distillation to obtain a high-activity epoxy-type crosslinking agent. The chemical structure of the high-activity epoxy-type crosslinking agent is as follows:
[0036]
[0037] The preparation method of the polymer amphiphilic emulsifier in the following embodiments of the present invention is as follows:
[0038] Under nitrogen protection, 60g of β-carboxyethyl acrylate, 80g of ethanol, 2g of 2-cyano-2-propylbenzodisulfide (CAS: 201611-85-0) and 0.8g of azobisisobutyronitrile were added to the reactor, stirred and reacted at a constant temperature of 60°C for 12h, and then 20g of o-phenylphenoxyethyl acrylate and 2.2g of azobisisobutyronitrile were added to the reaction system, and stirred and reacted at a constant temperature of 60°C for 12h, and then AMP-95 was added to the reaction system for neutralization reaction, so that the pH of the reaction system was 7, and finally the solvent was removed by vacuum at 65°C to obtain β-hydroxyethyl acrylate-o-phenylphenoxyethyl acrylate amphiphilic block polymer, i.e., polymer amphiphilic emulsifier.
[0039] The curing agent in the following embodiments of the present invention is an organosilicon crosslinking agent Silicone-9301, which is purchased from Beijing Baiyuan Chemical Co., Ltd.
[0040] The reducing agent in the following examples of the present invention is Bruggolite FF6M.
[0041] Example 1
[0042] An ultra-low viscosity water-based pressure-sensitive adhesive for a polarizer, comprising a resin composition and a curing agent, wherein the mass ratio of the resin composition to the curing agent is 100:3;
[0043] The resin composition, in parts by weight, comprises the following raw materials:
[0044]
[0045] The cross-linking monomer is tripropylene glycol diacrylate.
[0046] The initiator is potassium persulfate.
[0047] The preparation method of the ultra-low viscosity water-based pressure-sensitive adhesive for polarizer is as follows:
[0048] (1) After fully mixing a highly active epoxy crosslinking agent, butyl acrylate, styrene, acrylic acid, and a crosslinking monomer according to the formula amount, the mixture is then mixed with 13 / 25 of the formula amount of deionized water, butadiene, 3 / 5 of the formula amount of an initiator, n-dodecyl mercaptan, and a polymer amphiphilic emulsifier, and the mixture is stirred at high speed and emulsified under pressure to obtain a monomer pre-emulsion;
[0049] (2) The remaining amount of deionized water is heated to 80°C, 5% of the total mass of the monomer pre-emulsion obtained in step (1) and the remaining initiator are added, and the reaction is stirred at a constant temperature for 20 minutes at 0.3 MPa, and then the remaining monomer pre-emulsion is added dropwise within 3 hours, and the stirring is continued at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 60°C, and the reducing agent is added dropwise to the reaction system while stirring, and the dropping time is controlled within 30 minutes. After the dropping is completed, the reaction is stirred at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 25°C, and the pH value adjusting agent is added to make the pH of the reaction system = 7. After stirring evenly, the material is filtered to obtain an ultra-low viscosity water-based pressure-sensitive adhesive for polarizer. The pH value adjusting agent is ammonia water with a mass concentration of 25%.
[0050] Example 2
[0051] An ultra-low viscosity water-based pressure-sensitive adhesive for a polarizer, comprising a resin composition and a curing agent, wherein the mass ratio of the resin composition to the curing agent is 100:3.5;
[0052] The resin composition, in parts by weight, comprises the following raw materials:
[0053]
[0054] The crosslinking monomer is trimethylolpropane triacrylate.
[0055] The initiator is ammonium persulfate.
[0056] The preparation method of the ultra-low viscosity water-based pressure-sensitive adhesive for polarizer is as follows:
[0057] (1) After fully mixing a highly active epoxy crosslinking agent, butyl acrylate, styrene, acrylic acid, and a crosslinking monomer according to the formula amount, the mixture is then mixed with 13 / 25 of the formula amount of deionized water, butadiene, 3 / 5 of the formula amount of an initiator, n-dodecyl mercaptan, and a polymer amphiphilic emulsifier, and the mixture is stirred at high speed and emulsified under pressure to obtain a monomer pre-emulsion;
[0058] (2) The remaining amount of deionized water is heated to 80°C, 6% of the total mass of the monomer pre-emulsion obtained in step (1) and the remaining initiator are added, and the reaction is stirred at a constant temperature of 0.5 MPa for 20 minutes, and then the remaining monomer pre-emulsion is added dropwise within 4 hours, and the stirring is continued at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 62°C, and the reducing agent is added dropwise to the reaction system while stirring, and the dropping time is controlled within 35 minutes. After the dropwise addition is completed, the reaction is stirred at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 25°C, and the pH value adjusting agent is added to make the pH of the reaction system = 7. After stirring evenly, the material is filtered to obtain an ultra-low viscosity water-based pressure-sensitive adhesive for polarizer. The pH value adjusting agent is ammonia water with a mass concentration of 26%.
[0059] Example 3
[0060] An ultra-low viscosity water-based pressure-sensitive adhesive for a polarizer, comprising a resin composition and a curing agent, wherein the mass ratio of the resin composition to the curing agent is 100:4;
[0061] The resin composition, in parts by weight, comprises the following raw materials:
[0062]
[0063] The cross-linking monomer is 1,6-hexanediol diacrylate.
[0064] The initiator is potassium persulfate.
[0065] The preparation method of the ultra-low viscosity water-based pressure-sensitive adhesive for polarizer is as follows:
[0066] (1) After fully mixing a highly active epoxy crosslinking agent, butyl acrylate, styrene, acrylic acid, and a crosslinking monomer according to the formula amount, the mixture is then mixed with 13 / 25 of the formula amount of deionized water, butadiene, 3 / 5 of the formula amount of an initiator, n-dodecyl mercaptan, and a polymer amphiphilic emulsifier, and the mixture is stirred at high speed and emulsified under pressure to obtain a monomer pre-emulsion;
[0067] (2) The remaining amount of deionized water is heated to 80°C, 7% of the total mass of the monomer pre-emulsion obtained in step (1) and the remaining initiator are added, and the reaction is stirred at a constant temperature of 0.8 MPa for 20 minutes, and then the remaining monomer pre-emulsion is added dropwise within 5 hours, and the stirring is continued at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 65°C, and the reducing agent is added dropwise to the reaction system while stirring, and the dropping time is controlled within 45 minutes. After the dropwise addition is completed, the reaction is stirred at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 25°C, and the pH value adjusting agent is added to make the pH of the reaction system = 7. After stirring evenly, the material is filtered to obtain an ultra-low viscosity water-based pressure-sensitive adhesive for polarizer. The pH value adjusting agent is ammonia water with a mass concentration of 28%.
[0068] Example 4
[0069] An ultra-low viscosity water-based pressure-sensitive adhesive for a polarizer, comprising a resin composition and a curing agent, wherein the mass ratio of the resin composition to the curing agent is 100:4.5;
[0070] The resin composition, in parts by weight, comprises the following raw materials:
[0071]
[0072] The cross-linking monomer is tripropylene glycol diacrylate.
[0073] The initiator is potassium persulfate.
[0074] The preparation method of the ultra-low viscosity water-based pressure-sensitive adhesive for polarizer is as follows:
[0075] (1) After fully mixing a highly active epoxy crosslinking agent, butyl acrylate, styrene, acrylic acid, and a crosslinking monomer according to the formula amount, the mixture is then mixed with 13 / 25 of the formula amount of deionized water, butadiene, 3 / 5 of the formula amount of an initiator, n-dodecyl mercaptan, and a polymer amphiphilic emulsifier, and the mixture is stirred at high speed and emulsified under pressure to obtain a monomer pre-emulsion;
[0076] (2) The remaining amount of deionized water is heated to 80°C, 8% of the total mass of the monomer pre-emulsion obtained in step (1) and the remaining initiator are added, and the reaction is stirred at a constant temperature for 20 minutes at 1 MPa, and then the remaining monomer pre-emulsion is added dropwise within 5 hours, and the stirring is continued at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 65°C, and the reducing agent is added dropwise to the reaction system while stirring, and the dropping time is controlled within 45 minutes. After the dropwise addition is completed, the reaction is stirred at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 25°C, and the pH value adjusting agent is added to make the pH of the reaction system = 7. After stirring evenly, the material is filtered to obtain an ultra-low viscosity water-based pressure-sensitive adhesive for polarizer. The pH value adjusting agent is ammonia water with a mass concentration of 25%.
[0077] Example 5
[0078] An ultra-low viscosity water-based pressure-sensitive adhesive for a polarizer, comprising a resin composition and a curing agent, wherein the mass ratio of the resin composition to the curing agent is 100:5;
[0079] The resin composition, in parts by weight, comprises the following raw materials:
[0080]
[0081]
[0082] The cross-linking monomer is 1,6-hexanediol diacrylate.
[0083] The initiator is ammonium persulfate.
[0084] The preparation method of the ultra-low viscosity water-based pressure-sensitive adhesive for polarizer is as follows:
[0085] (1) After fully mixing a highly active epoxy crosslinking agent, butyl acrylate, styrene, acrylic acid, and a crosslinking monomer according to the formula amount, the mixture is then mixed with 13 / 25 of the formula amount of deionized water, butadiene, 3 / 5 of the formula amount of an initiator, n-dodecyl mercaptan, and a polymer amphiphilic emulsifier, and the mixture is stirred at high speed and emulsified under pressure to obtain a monomer pre-emulsion;
[0086] (2) The remaining amount of deionized water is heated to 80°C, 7% of the total mass of the monomer pre-emulsion obtained in step (1) and the remaining initiator are added, and the reaction is stirred at a constant temperature for 20 minutes at 0.3 MPa, and then the remaining monomer pre-emulsion is added dropwise within 3 hours, and the stirring is continued at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 60°C, and the reducing agent is added dropwise to the reaction system while stirring, and the dropping time is controlled within 30 minutes. After the dropwise addition is completed, the reaction is stirred at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 25°C, and the pH value adjusting agent is added to make the pH of the reaction system = 7. After stirring evenly, the material is filtered to obtain an ultra-low viscosity water-based pressure-sensitive adhesive for polarizer. The pH value adjusting agent is ammonia water with a mass concentration of 25%.
[0087] Comparative Example 1 is the same as Example 1, except that the high-activity epoxy crosslinking agent in Example 1 is replaced by an equal weight portion of a tetrafunctional epoxy resin in Comparative Example 1, and the tetrafunctional epoxy resin is prepared according to the following steps:
[0088] (1) 4,4'-diphenylsulfone diamine and excess epichlorohydrin are added to anhydrous ethanol, and the mixture is stirred at a constant temperature of 30-50°C to react. The reaction is monitored by FTIR. When the absorption peak of the amino group disappears in the infrared spectrum, the reaction is completed. After the reaction is completed, the excess epichlorohydrin is removed by vacuum distillation to obtain an intermediate product I. The chemical structure of the intermediate product I is as follows:
[0089]
[0090] (2) Then, alkali is added dropwise to the above reaction system while stirring, and the reaction is stirred at a constant temperature of 35-70° C., and the reaction is monitored by FTIR. When the absorption peak of the epoxy group in the infrared spectrum no longer increases, the addition of alkali is stopped and the reaction is terminated. Then, methyl isobutyl ketone and deionized water are added to the reaction system of step (2), and after stirring evenly, liquid separation and extraction are performed to remove the water layer, and a sodium hydroxide aqueous solution with a mass concentration of 10-15% is added to the remaining extract, and the volume ratio of the sodium hydroxide aqueous solution to the remaining extract is 1:2. Then, the reaction is stirred at a constant temperature of 50-65° C. for 1-3 hours, and then the reaction solution is washed with a sodium chloride aqueous solution until it is neutral, and the solvent is removed by reduced pressure distillation to obtain a tetrafunctional epoxy resin. The alkali is a NaOH aqueous solution with a mass concentration of 40%, and the mass concentration of the sodium chloride aqueous solution is 2-8%. The chemical structure of the tetrafunctional epoxy resin is as follows:
[0091]
[0092] Comparative Example 2 is the same as Example 1, except that the preparation method of the polymer amphiphilic emulsifier in Comparative Example 2 is as follows:
[0093] Under nitrogen protection, 60 g of β-carboxyethyl acrylate, 80 g of ethanol, 2 g of 2-cyano-2-propylbenzodisulfide (CAS: 201611-85-0), and 0.8 g of azobisisobutyronitrile were added to the reactor, stirred and reacted at a constant temperature of 60° C. for 12 h, and then 20 g of benzyl methacrylate and 2.2 g of azobisisobutyronitrile were added to the reaction system, and stirred and reacted at a constant temperature of 60° C. for 12 h, and then AMP-95 was added to the reaction system for neutralization reaction, so that the pH of the reaction system was 7, and finally the solvent was removed by vacuum at 65° C. to obtain β-hydroxyethyl acrylate-benzyl methacrylate amphiphilic block polymer, i.e., a polymer amphiphilic emulsifier.
[0094] Comparative Example 3 is the same as Example 1, except that the preparation method of the polymer amphiphilic emulsifier in Comparative Example 3 is as follows:
[0095] Under nitrogen protection, 60 g of β-carboxyethyl acrylate, 80 g of ethanol, 2 g of 2-cyano-2-propylbenzodisulfide (CAS: 201611-85-0) and 0.8 g of azobisisobutyronitrile were added to the reactor, stirred and reacted at a constant temperature of 60° C. for 12 h, and then 20 g of butyl acrylate and 2.2 g of azobisisobutyronitrile were added to the reaction system, and stirred and reacted at a constant temperature of 60° C. for 12 h, and then AMP-95 was added to the reaction system for neutralization reaction, so that the pH of the reaction system was 7, and finally the solvent was removed by vacuum at 65° C. to obtain β-hydroxyethyl acrylate-butyl acrylate amphiphilic block polymer, i.e., polymer amphiphilic emulsifier.
[0096] Comparative Example 4 is the same as Example 1, except that the preparation method of the polymer amphiphilic emulsifier in Comparative Example 4 is as follows:
[0097] Under nitrogen protection, 60g of acrylic acid, 80g of ethanol, 2g of 2-cyano-2-propylbenzodisulfide (CAS: 201611-85-0) and 0.8g of azobisisobutyronitrile were added to the reactor, stirred and reacted at a constant temperature of 60°C for 12h, and then 20g of o-phenylphenoxyethyl acrylate and 2.2g of azobisisobutyronitrile were added to the reaction system, and stirred and reacted at a constant temperature of 60°C for 12h, and then AMP-95 was added to the reaction system for neutralization reaction, so that the pH of the reaction system was 7, and finally the solvent was removed by vacuum at 65°C to obtain an acrylic acid-o-phenylphenoxyethyl acrylate amphiphilic block polymer, i.e., a polymer amphiphilic emulsifier.
[0098] Comparative Example 5 is the same as Example 1, except that Comparative Example 5 is a water-based pressure-sensitive adhesive of a pure acrylic emulsion system, which is composed of a resin composition and a curing agent, and the mass ratio of the resin composition to the curing agent is 100:3.5;
[0099] The resin composition, in parts by weight, comprises the following raw materials:
[0100]
[0101] The crosslinking monomer is trimethylolpropane triacrylate.
[0102] The initiator is ammonium persulfate.
[0103] The preparation method of the ultra-low viscosity water-based pressure-sensitive adhesive for polarizer is as follows:
[0104] (1) After fully mixing a high-activity epoxy crosslinking agent, butyl acrylate, methyl methacrylate, isooctyl acrylate, acrylic acid, and a crosslinking monomer according to the formula amount, the mixture is then mixed with 13 / 25 of a formula amount of deionized water, 3 / 5 of a formula amount of an initiator, n-dodecyl mercaptan, and a polymer amphiphilic emulsifier, and stirred at high speed to emulsify to obtain a monomer pre-emulsion;
[0105] (2) The remaining amount of deionized water is heated to 80°C, 6% of the total mass of the monomer pre-emulsion obtained in step (1) and the remaining initiator are added, and the reaction is stirred at a constant temperature of 0.5 MPa for 20 minutes, and then the remaining monomer pre-emulsion is added dropwise within 4 hours, and the stirring is continued at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 62°C, and the reducing agent is added dropwise to the reaction system while stirring, and the dropping time is controlled within 35 minutes. After the dropwise addition is completed, the reaction is stirred at a constant temperature for 1 hour, and then the temperature of the reaction system is reduced to 25°C, and the pH value adjusting agent is added to make the pH of the reaction system = 7. After stirring evenly, the material is filtered to obtain an ultra-low viscosity water-based pressure-sensitive adhesive for polarizer. The pH value adjusting agent is ammonia water with a mass concentration of 26%.
[0106] Performance Testing
[0107] The resin compositions and curing agents in Examples 1-5 of the present invention and Comparative Examples 1-5 were mixed evenly according to the formula amount to obtain water-based pressure-sensitive adhesives, which were coated on PET polyester films with a thickness of 40 μm. The film thickness was 8 μm, and a release film was covered on the surface of the film to obtain pressure-sensitive adhesive film samples. The pressure-sensitive adhesive film samples obtained in Examples 1-5 of the present invention and Comparative Examples 1-5 were tested for relevant properties, and the specific test results are shown in Table 1.
[0108] Adhesive surface resistance test: Cut the pressure-sensitive adhesive film sample into 12×12mm size, remove the release film, and then cure it at 80℃ for 2 minutes. Then test the adhesive surface resistance on a high resistance meter (model: SME-8310). The higher the adhesive surface resistance, the higher the film tearing voltage. 10 Ω can meet the use requirements.
[0109] Light transmittance and haze test: Referring to the standard GB / T2410-2008, using a haze meter (model: U3000), the release film of the pressure-sensitive adhesive film sample was torn off, and after curing at 80°C for 2 minutes, the light transmittance and haze of the material were measured.
[0110] 180° peel strength: According to GB / T2792-1995 “Test method for 180° peel strength of pressure-sensitive adhesive tapes”, the test was carried out using an electronic universal testing machine (the bonded material was a standard test steel plate, and the peeling rate was 300 mm / min).
[0111] 180° peel strength climb: remove the release film, stick the film to the steel plate, place it in a 70°C oven for 48 hours, and then measure it using an electronic universal testing machine in accordance with GB / T2792-1995 "Test method for 180° peel strength of pressure-sensitive adhesive tapes" (the bonded material is a standard test steel plate, and the peeling rate is 300 mm / min).
[0112] Table 1
[0113]
[0114] The surface resistance of the pressure-sensitive adhesive obtained in Comparative Example 1 is relatively large because the tetrafunctional epoxy resin in Comparative Example 1 does not undergo a cross-linking reaction with the carboxyl group at room temperature, while the high-activity epoxy cross-linking agent in Example 1 can undergo a cross-linking and curing reaction with the carboxyl group at room temperature, further increasing the cross-linking density of the pressure-sensitive adhesive layer. At the same time, the density of the high-activity epoxy cross-linking agent is greater than the density of the monomer for preparing the styrene-butadiene emulsion. At the same time, the carboxyl group in the latex system reacts to generate a hydroxyl group, which is also hydrophilic, which is beneficial to reducing the resistance value of the glue volume resistance and the surface resistance of the pressure-sensitive adhesive layer. The obtained pressure-sensitive adhesive layer has a better antistatic effect, and the film tearing voltage is further reduced.
[0115] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. An ultra-low viscosity water-based pressure-sensitive adhesive for polarizer, characterized in that: It comprises a resin composition and a curing agent, wherein the mass ratio of the resin composition to the curing agent is 100:3-5; The resin composition, in parts by weight, comprises the following raw materials: The polymer amphiphilic emulsifier is a β-carboxyethyl acrylate-o-phenylphenoxyethyl acrylate amphiphilic block polymer, and the preparation method of the polymer amphiphilic emulsifier comprises the following steps: Under nitrogen protection, 60g of β-carboxyethyl acrylate, 80g of ethanol, 2g of 2-cyano-2-propylbenzodisulfide, and 0.8g of azobisisobutyronitrile are added to a reactor, and stirred at a constant temperature of 60°C for 12-24h. Then, 20g of o-phenylphenoxyethyl acrylate and 2.2g of azobisisobutyronitrile are added to the reaction system, and stirred at a constant temperature of 60°C for 12-24h. Then, AMP-95 is added to the reaction system for neutralization reaction, so that the pH of the reaction system is 7. Finally, the solvent is removed by vacuum at 65°C to obtain a β-hydroxyethyl acrylate-o-phenylphenoxyethyl acrylate amphiphilic block polymer, i.e., a polymer amphiphilic emulsifier; The highly active epoxy crosslinking agent contains 8 epoxy groups in its molecular structure.
2. The ultra-low viscosity water-based pressure-sensitive adhesive for polarizer according to claim 1, characterized in that: The preparation method of the highly active epoxy crosslinking agent comprises the following steps: (1) 1,2,4,5-benzenetetraamine and excess epichlorohydrin are added to anhydrous ethanol, and the mixture is stirred at a constant temperature of 30-50° C. The reaction is monitored by FTIR. When the absorption peak of the amino group disappears in the infrared spectrum, the reaction is completed. After the reaction is completed, the excess epichlorohydrin is removed by vacuum distillation to obtain an intermediate product I. The chemical structure of the intermediate product I is as follows: (2) Then, alkali is added dropwise to the above reaction system while stirring, and the reaction is stirred at a constant temperature of 35-70° C., and the progress of the reaction is monitored by FTIR. When the absorption peak of the epoxy group in the infrared spectrum no longer increases, the addition of alkali is stopped, and the reaction is terminated. Then, methyl isobutyl ketone and deionized water are added to the reaction system of step (2), and after stirring evenly, liquid separation and extraction are performed, and the water layer is removed. The remaining extract is placed at a constant temperature of 50-65° C. and stirred for 1-3 hours. Then, the reaction solution is washed with sodium chloride aqueous solution until it is neutral, and the solvent is removed by reduced pressure distillation to obtain a high-activity epoxy-type crosslinking agent. The chemical structure of the high-activity epoxy-type crosslinking agent is as follows:
3. The ultra-low viscosity water-based pressure-sensitive adhesive for polarizer according to claim 2, characterized in that: The alkali in step (2) is a NaOH aqueous solution or a KOH aqueous solution with a mass concentration of 15-40%.
4. The ultra-low viscosity water-based pressure-sensitive adhesive for polarizer according to claim 2, characterized in that: The mass concentration of the sodium chloride aqueous solution is 2-8%.
5. The ultra-low viscosity water-based pressure-sensitive adhesive for polarizer according to claim 1, characterized in that: The cross-linking monomer includes at least one of tripropylene glycol diacrylate, trimethylolpropane triacrylate, and 1,6-hexanediol diacrylate.
6. The ultra-low viscosity water-based pressure-sensitive adhesive for polarizer according to claim 1, characterized in that: The curing agent is an organic silicon cross-linking agent Silicone-9301, purchased from Beijing Baiyuan Chemical Co., Ltd.
7. The ultra-low viscosity water-based pressure-sensitive adhesive for polarizer according to claim 1, characterized in that: The initiator includes potassium persulfate or ammonium persulfate.
8. The ultra-low viscosity water-based pressure-sensitive adhesive for polarizer according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) After fully mixing a highly active epoxy crosslinking agent, butyl acrylate, styrene, acrylic acid, and a crosslinking monomer according to the formula amount, the mixture is then mixed with 13 / 25 of the formula amount of deionized water, butadiene, 3 / 5 of the formula amount of an initiator, n-dodecyl mercaptan, and a polymer amphiphilic emulsifier, and the mixture is stirred at high speed and emulsified under pressure to obtain a monomer pre-emulsion; (2) heating the remaining amount of deionized water to 80° C., adding 5-8% of the total mass of the monomer pre-emulsion obtained in step (1) and the remaining initiator, stirring and reacting at a constant temperature of 0.3-1 MPa for 20 min, then dropping the remaining amount of monomer pre-emulsion within 3-5 h, stirring at a constant temperature for 1 h, then reducing the temperature of the reaction system to 60-65° C., and starting to drop the reduced agent into the reaction system while stirring, the dropping time is controlled within 30-45 min. After the dropwise addition is completed, stirring and reacting at a constant temperature for 1 h, then reducing the temperature of the reaction system to below 25° C., adding the pH adjuster in the formula amount so that the pH of the reaction system is 7-8, stirring evenly, filtering and discharging the material, and obtaining an ultra-low viscosity water-based pressure-sensitive adhesive for polarizer.