Halogen-free flame-retardant low-density polyurethane sealant and preparation method thereof

Through the specific ratio of halogen-free flame-retardant low-density polyurethane sealant, combined with nano-grade lightweight fillers and liquid flame retardants, the shortcomings in the comprehensive performance of polyurethane sealant in the prior art are solved, and low density and high resistance are achieved Fuelability and good mechanical properties are suitable for rail transit and automotive interiors.

CN118909588APending Publication Date: 2024-11-08BEIJING FROST MOON TECH CO LTD

Patent Information

Application Number
CN202411208222.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing polyurethane sealants have not yet met the needs of applications such as rail transit and automotive interiors in terms of comprehensive performance, especially in terms of flame retardancy, density and mechanical properties.

Method used

Halogen-free flame-retardant low-density polyurethane sealant is used, and it is composed of components A and components B in specific proportions, including modified polyether polyols, plasticizers, tougheners, chain extenders, catalysts, and thickeners , defoaming agent, coupling agent, filler and flame retardant, combined with nano-grade light filler and liquid flame retardant, to achieve room temperature curing and low density characteristics.

Benefits of technology

It has achieved low curing temperature, strong thixotropy, good elasticity, light weight and halogen-free flame retardant properties. The density is in the range of 0.4-0.6 g/cm3 and the oxygen index is ≥35%. It is suitable for rail transit and automotive interiors and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of sealant materials, in particular to a halogen-free flame-retardant low-density polyurethane sealant and a preparation method thereof. The halogen-free flame-retardant low-density polyurethane sealant disclosed by the invention is prepared from a component A and a component B, the component A comprises the following raw materials: modified polyether polyol, a plasticizer, a flexibilizer, a chain extender, a catalyst, a thickening agent, a defoaming agent, a coupling agent, a filler and a flame retardant; and the component B comprises the following raw materials: polyisocyanate, a coupling agent, a thickening agent and a filler. The halogen-free flame-retardant low-density polyurethane sealant provided by the invention can be completely cured at room temperature for 48 hours, has the characteristics of low curing temperature, strong thixotropy and no flowing, and has the advantages of low raw material cost, simple preparation method and excellent market prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealants, and in particular to a halogen-free flame-retardant low-density polyurethane sealant and a preparation method thereof. Background Art

[0002] Two-component polyurethane adhesive is the most important category of polyurethane adhesives, with a wide range of uses and large dosage. It is usually composed of two components, A and B, which are packaged separately and can be prepared in a certain proportion before use. Component A (main agent) is a hydroxyl component, and component B (curing agent) is a component containing free isocyanate groups. Components A and B are mixed in a certain proportion to form polyurethane resin.

[0003] Polyurethane sealants have excellent elasticity, low temperature resistance, wear resistance and good adhesion to substrates. Therefore, they are widely used in construction, automobiles, home decoration, waterproofing and shipbuilding. Two-component polyurethane adhesives can usually be cured at room temperature, and the curing speed can be adjusted by selecting the raw materials for preparing the adhesive or adding catalysts. Its bonding strength is greater than that of single-component adhesives and can meet the requirements of structural adhesives. The dosage of the two components can be adjusted within a certain range, and there is generally a certain tolerance. The NCO / OH molar ratio can be less than 1 or greater than 1 several times. When the NCO component (curing agent) is excessive, the polyisocyanate self-polymerizes to form a tough adhesive layer, which is suitable for the bonding of hard materials; when the NCO component is used in small amounts, the adhesive layer is soft and can be used for the bonding of soft materials such as leather and fabrics. Since its advent, two-component polyurethane adhesives have become the product with the most varieties and the largest output among polyurethane adhesives due to their advantages such as adjustable performance, high bonding strength and wide bonding range. Polyurethane sealants are flammable and need to be flame retardant. Halogen-free flame retardants are available in powder and liquid forms. Powder flame retardants are easy to migrate and have a high density, which will increase the weight of the polyurethane sealant. For this reason, hollow fillers and thickeners are used to improve the migration of powder flame retardants and reduce density.

[0004] Chinese application CN115074073A discloses "a flame retardant polyurethane sealant and its preparation method", which improves flame retardancy by adding flame retardant elements chlorine and nitrogen through chemical reaction. Chinese application CN117025160A discloses "a heat-resistant polyurethane sealant and its preparation method", which uses polyurethane plasticizers terminated with organosilicon ether room temperature ionic liquids to improve the heat resistance of the sealant, effectively inhibit the migration of conventional plasticizers, and improve the mechanical properties of the sealant. Although the mechanical properties of the above two types of polyurethane sealants are acceptable, their comprehensive performance still needs to be further significantly improved. Summary of the invention

[0005] The present invention aims to address the deficiencies of current technologies and to propose a halogen-free flame-retardant low-density polyurethane sealant and a preparation method thereof according to application requirements such as rail transit and automobile interior sealing. The halogen-free flame-retardant low-density polyurethane sealant can be cured at room temperature, is easy to operate, has low curing temperature, strong thixotropy, good elasticity after curing, is light in weight, and has the characteristics of being halogen-free and flame-retardant.

[0006] Specifically, the present invention provides a halogen-free flame-retardant low-density polyurethane sealant, which includes component A and component B, wherein the component A includes the following raw materials in weight ratio: 60-90 parts of modified polyether polyol; 2-10 parts of plasticizer, 10-25 parts of toughening agent, 10-20 parts of chain extender, 0.1-0.5 parts of catalyst, 1-5 parts of thickener, 0.5-1.5 parts of defoamer, 1-5 parts of coupling agent, 10-30 parts of filler, 5-30 parts of flame retardant; the modified polyether polyol is composed of biopolyol and polyether polyol in a dosage ratio of 1:1-1.5; The B component comprises the following raw materials in weight ratio: 10-20 parts of polyisocyanate, 1-5 parts of coupling agent, 1-5 parts of thickener, 10-30 parts of filler and 10-30 parts of flame retardant.

[0007] In the halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the weight ratio of the component A to the component B is (1-1.5):0.5; preferably (1-1.2):0.5.

[0008] In a preferred embodiment of the present invention, the component A is composed of the following raw materials in the following weight ratio: 60-80 parts of modified polyether polyol; 4-8 parts of plasticizer, 15-20 parts of toughening agent, 10-15 parts of chain extender, 0.1-0.3 parts of catalyst, 2-4 parts of thickener, 0.6-1.0 parts of defoamer, 2-4 parts of coupling agent, 12-25 parts of filler, and 15-25 parts of flame retardant; the modified polyether polyol is composed of biopolyol and polyether polyol in a dosage ratio of 1:1.

[0009] In a preferred embodiment of the present invention, the B component is composed of raw materials in the following weight ratios: 12-18 parts of polyisocyanate, 2-4 parts of coupling agent, 2-4 parts of thickener, 12-25 parts of filler, and 15-25 parts of flame retardant.

[0010] In the halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the biopolyol is one or a combination of castor oil, modified castor oil, soybean oil and palm oil.

[0011] Preferably, the biopolyol is one of castor oil, modified castor oil or soybean oil.

[0012] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention comprises polyether polyols selected from polyether polyols with a functionality of 2 or 3 and polyether polyols with a molecular weight of 500-3000, or a combination of several thereof, preferably polyether polyols with a molecular weight of 500 or 1000.

[0013] Suitable specific combinations include castor oil and polyether polyol with a molecular weight of 500, modified castor oil and polyether polyol with a molecular weight of 1000, soybean oil and polyether polyol with a molecular weight of 500, and the like.

[0014] The polyether polyol described in the present invention is particularly preferably a polyether polyol having a functionality of 3 and a molecular weight of 1000.

[0015] The present invention selects the modified polyether polyol to improve flexibility and hardness and has the advantage of low temperature resistance.

[0016] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention comprises a plasticizer selected from diisononyl phthalate, dibutyl phthalate, acetylcitrate tributyl dioctyl dicarboxylate, triphenyl phosphate, dibutyl sebacate, and dioctyl sebacate, or a combination of several thereof.

[0017] Preferably, the plasticizer is one or two selected from diisononyl phthalate, dibutyl phthalate, and triphenyl phosphate, more preferably one.

[0018] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, wherein the toughening agent is hydroxyl-terminated polybutadiene or hydroxyl-terminated nitrile rubber, preferably hydroxyl-terminated polybutadiene. By using the above toughening agent, the toughness can be improved, and the advantages of fatigue resistance and impact resistance can be obtained.

[0019] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the chain extender is selected from 1,4-butanediol, ethylene glycol, 1,6-hexanediol, pentanediol, trimethylolpropane, hydroquinone dihydroxyethyl ether, resorcinol dihydroxyethyl ether, di-o-chlorodiphenylamine (MOCA), dimethylthiotoluene diamine (E300), 2,4-diamino-3,5-dimethylthiochlorobenzene (TX-2), 2,4-diamino-5-mercaptotoluene (TX-1), 4,4'-methylene-bis(3-chloro-2,6-diethylaniline (MCDEA), 4,4 '-diaminodiphenylmethane (MDA) or a combination thereof. Preferably, the chain extender is selected from 1,4-butanediol, ethylene glycol, 1,6-hexanediol, pentanediol or a combination thereof, preferably one. The chain extender selected from the present invention can improve the binding force between the modified polyol and the isocyanate, and has the advantages of heat resistance and moisture absorption resistance.

[0020] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the catalyst is selected from one or a combination of stannous octoate, dioctyltin dilaurate, dimethyltin dilaurate, dibutyltin dilaurate, butyltin oxide, octyltin oxide and triethanolamine. Preferably, the catalyst is selected from stannous octoate or dibutyltin dilaurate (also known as dibutyltin dilaurate).

[0021] In the halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the thickener in component A and the thickener in component B may be the same or different, and the thickener is one selected from fumed silica, hydrogenated castor oil and hydrated aluminum silicate, preferably fumed silica.

[0022] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention comprises the defoaming agent which is at least one selected from polydimethylsiloxane, fluorosilicone and glycol siloxane, preferably polydimethylsiloxane.

[0023] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the coupling agent is selected from one or a combination of r-methacryloxypropyltrimethoxysilane (KH570), r-glycidoxypropyltrimethoxysilane (KH560), r-aminopropyltriethoxysilane (KH550); preferably, the coupling agent is selected from r-glycidoxypropyltrimethoxysilane (KH560) or r-aminopropyltriethoxysilane (KH550).

[0024] In a specific embodiment of the present invention, the coupling agent in the A component and the coupling agent in the B component may be the same or different.

[0025] In a preferred embodiment of the present invention, the coupling agent in the A component is KH560.

[0026] In a preferred embodiment of the present invention, the coupling agent in the B component is KH550.

[0027] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention comprises a filler selected from one or a combination of organic modified bentonite, hollow glass microspheres, hollow phenolic resin, ceramic hollow microspheres, pulverized coal hollow microspheres, hollow carbon microspheres and one or a combination of nano-scale light calcium carbonate, nano-talc powder, nano-silicon powder and nano-titanium dioxide; preferably, the filler is a mixture of organic modified bentonite, hollow glass microspheres or hollow phenolic resin and nano-scale light calcium carbonate.

[0028] In the halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the filler in the component A and the filler in the component B may be the same as or different from each other.

[0029] In a preferred embodiment of the present invention, the filler in component A is a mixture of hollow glass microspheres / hollow phenolic resin and light calcium carbonate, and the appropriate dosage ratio is 3-4:1.

[0030] In a preferred embodiment of the present invention, the filler in the B component is a mixture of hollow glass microspheres / hollow phenolic resin and light calcium carbonate, and the appropriate dosage ratio is 3-4:1.

[0031] The filler selected by the present invention has the advantages of heat resistance and low density, which reduces the density of the product and makes it light.

[0032] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the flame retardant is a mixture of a liquid flame retardant and a powder flame retardant, and is selected from a combination of two or more of nano-scale aluminum hydroxide, nano-scale strong magnesium oxide, nano-scale ammonium polyphosphate, nano-scale melamine cyanurate, ammonium polyphosphate, trimethyl phosphate, trioctyl phosphate, and diphenylethylhexyl phosphate. Preferably, the flame retardant is a combination of two or more of nano-scale melamine cyanurate, ammonium polyphosphate, trimethyl phosphate, trioctyl phosphate, and diphenylethylhexyl phosphate; particularly prominent combinations include a combination of ammonium polyphosphate and trimethyl phosphate in a ratio of 2-3:1 or a combination of nano-scale melamine cyanurate and trioctyl phosphate in a ratio of 2-3:1.

[0033] In a preferred embodiment of the present invention, the flame retardant in the component A is a combination of nano-scale melamine cyanurate and trioctyl phosphate in a ratio of 2-3:1, and the appropriate dosage ratio is 3:1.

[0034] In a preferred embodiment of the present invention, the flame retardant in the B component is a combination of ammonium polyphosphate and trimethyl phosphate in a ratio of 2-3:1, and the appropriate dosage ratio is 2:1.

[0035] The use of the flame retardant can improve combustion resistance, reduce smoke density, and has the advantage of halogen-free flame retardancy.

[0036] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention, the isocyanate is selected from one or a combination of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), 1,6-hexanodioic acid diisocyanate (HDI), 1-isocyanate-3-isocyanatomethyl-3,5,5-trimethylcyclohexane (isophornon diisocyanate, IPDI) and 4,4'-diisocyanate dicyclohexylmethane; preferably, the isocyanate is selected from toluene diisocyanate (TDI) or diphenylmethane diisocyanate (MDI), which has more prominent reaction with polyol and improves hardness.

[0037] As the best embodiment of the present invention, the halogen-free flame-retardant low-density polyurethane sealant is composed of component A and component B in a weight ratio of (1-1.2):0.5: The raw materials of component A in weight proportion are as follows: 20-40 parts of castor oil; 20-40 parts of polyether polyol with a molecular weight of 500 or 1000; 4-8 parts of plasticizer diisononyl phthalate, 15-20 parts of toughening agent terminal hydroxyl polybutadiene, 10-15 parts of chain extender 1,4-butanediol, 0.1-0.3 parts of catalyst dibutyltin dilaurate, 2-4 parts of thickener fumed silica, 0.6-1.0 parts of defoaming agent polydimethylsiloxane, 2-4 parts of coupling agent r-glycidoxypropyltrimethylsilane (KH560), 10-20 parts of hollow phenolic resin filler, 2-5 parts of light calcium carbonate filler, 10-15 parts of nano-scale cyanuric acid melamine flame retardant, 5-10 parts of trioctyl phosphate flame retardant; The B component is composed of the following raw materials in the following weight ratios: 12-18 parts of diphenylmethane diisocyanate (MDI), 2-4 parts of coupling agent r-aminopropyltriethoxysilane (KH550), 2-4 parts of thickener fumed silica, 10-20 parts of hollow phenolic resin filler, 2-5 parts of light calcium carbonate filler, 10-15 parts of flame retardant ammonium polyphosphate, and 5-10 parts of flame retardant trimethyl phosphate.

[0038] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention has reasonable formula, excellent performance, low curing temperature, strong thixotropy, good elasticity after curing, light weight, halogen-free flame retardancy and the like, and has the advantages of excellent market prospects.

[0039] The halogen-free flame retardant low-density polyurethane sealant of the present invention can be prepared according to conventional knowledge in the art. However, in order to obtain a halogen-free flame retardant low-density polyurethane sealant with better performance, the present invention also provides a more ideal method for preparing the halogen-free flame retardant low-density polyurethane sealant.

[0040] In a specific embodiment of the present invention, a method for preparing a halogen-free flame-retardant low-density polyurethane sealant provided by the present invention comprises the following steps: (1) Biopolyol and polyether polyol in a ratio of 1:1-1.5 are mixed to form a modified polyether polyol. The modified polyether polyol, filler and powder flame retardant are stirred evenly and then dehydrated at 100-115°C for 4-6 hours. After cooling to below 80°C, plasticizer, toughening agent, chain extender, catalyst, thickener, defoamer, coupling agent and liquid flame retardant are added and stirred evenly to obtain component A; (2) Stir the filler and powder flame retardant at a high temperature of 100-115°C for dehydration for 4-6 hours; mix the isocyanate, coupling agent, thickener and filler, flame retardant (including powder flame retardant and liquid flame retardant, the same below), stir and mix evenly to obtain component B.

[0041] The method of the present invention preferably further comprises the steps of: (4) Mix component A and component B in a weight ratio of (1-1.5):0.5.

[0042] The preparation method is simple and convenient, has low preparation cost and is suitable for promotion.

[0043] The halogen-free flame-retardant low-density polyurethane sealant provided by the present invention can be completely cured at room temperature within 48 hours, and has the characteristics of low curing temperature, strong thixotropy, and no flow. Its various properties are as follows: (1) gel time at a temperature of 23°C±2°C is 50min-120min; (2) density is 0.4-0.6 g / cm3; (3) flame retardant performance is: oxygen index ≥35%. By optimizing the formula, the halogen-free flame-retardant low-density polyurethane sealant obtained by the present invention has excellent comprehensive performance and excellent market application prospects. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] All raw materials used in the following examples are known commercially available products. As for their optional sources, general raw materials from relevant raw material manufacturers can be used, for example, fumed silica is from Nantong Qianyi New Material Technology Co., Ltd., hollow phenolic resin is from Shengquan New Materials Co., Ltd., and diphenylmethane diisocyanate is from Shandong Bluestar Dongda Chemical Co., Ltd.

[0046] Example 1

[0047] This embodiment provides a halogen-free flame-retardant low-density polyurethane sealant, which is composed of component A and component B in a weight ratio of 1:0.5.

[0048] The raw materials of component A include, by weight proportion: 30 parts of castor oil, 30 parts of polyol with a molecular weight of 500, 8 parts of diisononyl phthalate, 20 parts of terminal hydroxyl polybutadiene, 10 parts of 1,4-butanediol, 0.1 parts of dibutyltin dilaurate, 4 parts of fumed silica, 0.8 parts of polydimethylsiloxane, 2 parts of r-glycidoxypropyltrimethoxysilane (KH560), 15 parts of hollow phenolic resin, 5 parts of light calcium carbonate, 15 parts of nano-grade melamine cyanurate, and 5 parts of trioctyl phosphate.

[0049] The raw materials of component B include, by weight, 15 parts of diphenylmethane diisocyanate (MDI), 2 parts of r-aminopropyltriethoxysilane (KH550), 2 parts of fumed silica, 10 parts of hollow phenolic resin, 3 parts of light calcium carbonate, 10 parts of ammonium polyphosphate, and 5 parts of trimethyl phosphate.

[0050] This embodiment also provides a method for preparing the above-mentioned halogen-free flame-retardant low-density polyurethane sealant, which is specifically as follows: (1) Preparation of component A: Castor oil, polyol with a molecular weight of 500, hollow phenolic resin, light calcium carbonate, and nano-scale cyanuric acid melamine are stirred evenly and then dehydrated at 110°C for 5 hours; the mixture is cooled to below 80°C and diisononyl phthalate, terminal hydroxyl polybutadiene, 1,4-butanediol, dibutyltin dilaurate, fumed silica, polydimethylsiloxane, r-glycidoxypropyltrimethylsilane (KH560), and trioctyl phosphate liquid flame retardant are added at once, and stirred evenly to obtain component A.

[0051] (2) Preparation of component B: dehydrating hollow phenolic resin, light calcium carbonate filler and ammonium polyphosphate at a high temperature of 110°C for 5 hours; stirring and mixing phenylmethane diisocyanate (MDI), r-aminopropyltriethoxysilane (KH550), hollow phenolic resin, light calcium carbonate fumed silica, trimethyl phosphate and ammonium polyphosphate to obtain component B.

[0052] (3) Mix component A and component B in a weight ratio of 1:0.5 and stir until the mixture is uniform.

[0053] Example 2

[0054] This embodiment provides a halogen-free flame-retardant low-density polyurethane sealant, which is composed of component A and component B in a weight ratio of 1:0.5.

[0055] The raw materials of component A include, by weight proportion: 30 parts of castor oil, 30 parts of polyol with a molecular weight of 1000, 8 parts of dibutyl phthalate, 20 parts of terminal hydroxyl polybutadiene, 10 parts of 1,6-hexanediol, 0.1 parts of dibutyl tin dilaurate, 4 parts of fumed silica, 0.8 parts of polydimethylsiloxane, 2 parts of r-glycidoxypropyltrimethoxysilane (KH560), 20 parts of hollow glass microspheres, 5 parts of light calcium carbonate, 15 parts of nano-scale melamine cyanurate, and 5 parts of trioctyl phosphate.

[0056] The raw materials of component B include, by weight: 15 parts of diphenylmethane diisocyanate (MDI), 2 parts of r-aminopropyltriethoxysilane (KH550), 2 parts of fumed silica, 10 parts of hollow glass microspheres, 3 parts of light calcium carbonate, 10 parts of ammonium polyphosphate, and 5 parts of trimethyl phosphate.

[0057] This embodiment also provides a method for preparing the above-mentioned halogen-free flame-retardant low-density polyurethane sealant, which is specifically as follows: (1) Preparation of component A: Castor oil, a polyol with a molecular weight of 1000, hollow glass microspheres, light calcium carbonate, and nano-scale melamine cyanurate are stirred evenly, and then dehydrated at 115°C for 4 hours; the mixture is cooled to below 80°C, and dibutyl phthalate, terminal hydroxyl polybutadiene, 1,6-hexanediol, dibutyltin dilaurate, fumed silica, polydimethylsiloxane, r-glycidoxypropyltrimethylsilane (KH560), nano-scale melamine cyanurate, and trioctyl phosphate liquid flame retardant are added at once, and stirred evenly to obtain component A.

[0058] (2) Preparation of component B: dehydrating hollow phenolic resin, light calcium carbonate filler and ammonium polyphosphate at a high temperature of 115°C for 4 hours; stirring and mixing phenylmethane diisocyanate (MDI), r-aminopropyltriethoxysilane (KH550), fumed silica, trimethyl phosphate, hollow phenolic resin, light calcium carbonate filler and ammonium polyphosphate to obtain component B.

[0059] (3) Mix component A and component B in a weight ratio of 1:0.5 and stir until the mixture is uniform.

[0060] Example 3

[0061] This embodiment provides a halogen-free flame-retardant low-density polyurethane sealant, which is composed of component A and component B in a weight ratio of 1:0.5.

[0062] The raw materials of component A in proportion by weight include: 30 parts of soybean oil, 30 parts of polyol with a molecular weight of 500, 8 parts of triphenyl phosphate, 20 parts of terminal hydroxy polybutadiene, 10 parts of ethylene glycol, 0.1 parts of stannous octoate, 4 parts of fumed silica, 0.8 parts of polydimethylsiloxane, 2 parts of r-glycidoxypropyltrimethoxysilane (KH560), 15 parts of hollow phenolic resin, 5 parts of light calcium carbonate, 15 parts of nano-grade melamine cyanurate, and 5 parts of trioctyl phosphate.

[0063] The raw materials of component B include, by weight, 15 parts of xylene diisocyanate (TDI), 2 parts of r-aminopropyltriethoxysilane (KH550), 2 parts of fumed silica, 0.8 parts of polydimethylsiloxane, 10 parts of hollow phenolic resin, 3 parts of light calcium carbonate, 10 parts of ammonium polyphosphate, and 5 parts of trimethyl phosphate.

[0064] This embodiment also provides a method for preparing the above-mentioned halogen-free flame-retardant low-density polyurethane sealant, which is specifically as follows: (1) Preparation of component A: Soybean oil, polyol with a molecular weight of 500, hollow phenolic resin, light calcium carbonate and nano-scale melamine cyanurate are mixed and then dehydrated at 100°C for 6 hours; the mixture is cooled to below 80°C and triphenyl phosphate, terminal hydroxyl polybutadiene, ethylene glycol, fumed silica, polydimethylsiloxane, r-glycidoxypropyltrimethylsilane (KH560), stannous octoate and trioctyl phosphate liquid flame retardant are added at once, and the mixture is mixed and then mixed to obtain component A.

[0065] (2) Preparation of component B: dehydrating hollow phenolic resin, light calcium carbonate filler and ammonium polyphosphate at 100°C for 6 hours; stirring and mixing toluene diisocyanate (TDI), r-aminopropyltriethoxysilane (KH550), fumed silica, polydimethylsiloxane, hollow phenolic resin, light calcium carbonate filler, ammonium polyphosphate and trimethyl phosphate to obtain component B.

[0066] (3) Mix component A and component B in a weight ratio of 1:0.5 and stir until the mixture is uniform.

[0067] Example 4

[0068] Compared with Example 1, the difference of this embodiment is only that the formula is different, specifically: This embodiment provides a halogen-free flame-retardant low-density polyurethane sealant, which is composed of component A and component B in a weight ratio of 1.5:0.5.

[0069] The raw materials of component A include, by weight proportion: 20 parts of castor oil, 40 parts of polyol with a molecular weight of 500, 6 parts of diisononyl phthalate, 15 parts of terminal hydroxyl polybutadiene, 15 parts of 1,4-butanediol, 0.3 parts of dibutyltin dilaurate, 2 parts of fumed silica, 1 part of polydimethylsiloxane, 4 parts of r-glycidoxypropyltrimethoxysilane (KH560), 20 parts of hollow phenolic resin, 5 parts of light calcium carbonate, 15 parts of nano-grade melamine cyanurate, and 10 parts of trioctyl phosphate.

[0070] The raw materials of component B include, by weight: 18 parts of diphenylmethane diisocyanate (MDI), 4 parts of r-aminopropyltriethoxysilane (KH550), 4 parts of fumed silica, 20 parts of hollow phenolic resin, 5 parts of light calcium carbonate, 15 parts of ammonium polyphosphate, and 10 parts of trimethyl phosphate.

[0071] Example 5

[0072] Compared with Example 1, the difference of this embodiment is only that the formula is different, specifically: This embodiment provides a halogen-free flame-retardant low-density polyurethane sealant, which is composed of component A and component B in a weight ratio of 1.2:0.5.

[0073] The raw materials of component A include, by weight proportion: 40 parts of castor oil, 20 parts of polyol with a molecular weight of 500, 4 parts of diisononyl phthalate, 15 parts of terminal hydroxyl polybutadiene, 12 parts of 1,4-butanediol, 0.2 parts of dibutyltin dilaurate, 2 parts of fumed silica, 0.6 parts of polydimethylsiloxane, 2 parts of r-glycidoxypropyltrimethoxysilane (KH560), 10 parts of hollow phenolic resin, 2 parts of light calcium carbonate, 11 parts of nano-grade melamine cyanurate, and 7 parts of trioctyl phosphate.

[0074] The raw materials of component B include, by weight: 12 parts of diphenylmethane diisocyanate (MDI), 2 parts of r-aminopropyltriethoxysilane (KH550), 2 parts of fumed silica, 15 parts of hollow phenolic resin, 2 parts of light calcium carbonate, 11 parts of ammonium polyphosphate, and 8 parts of trimethyl phosphate.

[0075] Comparative Example 1

[0076] This comparative example provides a halogen-free flame-retardant low-density polyurethane sealant, which is composed of component A and component B in a weight ratio of 1:0.5. The raw materials of component A in weight ratio include: 40 parts of polyol with a molecular weight of 500, 8 parts of diisononyl phthalate, 20 parts of terminal hydroxyl polybutadiene, 10 parts of 1,4-butanediol, 0.1 parts of dibutyltin dilaurate, 4 parts of fumed silica, 0.8 parts of polydimethylsiloxane, 2 parts of r-glycidoxypropyltrimethylsilane (KH560), 5 parts of light calcium carbonate, 15 parts of nano-grade melamine cyanurate, and 5 parts of trioctyl phosphate.

[0077] The raw materials of the B component include, by weight, 15 parts of diphenylmethane diisocyanate (MDI), 2 parts of r-aminopropyltriethoxysilane (KH550), 2 parts of fumed silica, and 3 parts of light calcium carbonate.

[0078] This comparative example also provides a preparation method of the above-mentioned halogen-free flame-retardant low-density polyurethane sealant, which is as follows: (1) Preparation of component A: A polyol with a molecular weight of 500 and light calcium carbonate are stirred evenly, and then dehydrated at a high temperature of 110°C for 5 hours; the temperature is lowered to below 80°C, and diisononyl phthalate, terminal hydroxy polybutadiene, 1,4-butanediol, dibutyltin dilaurate, fumed silica, polydimethylsiloxane, r-glycidoxypropyltrimethylsilane (KH560), nano-scale melamine cyanurate and trioctyl phosphate liquid flame retardant are added at once, and stirred evenly to obtain component A.

[0079] (2) Preparation of component B: Dehydrate the light calcium carbonate filler at a high temperature of 110°C for 5 hours; stir and mix phenylmethane diisocyanate (MDI), r-aminopropyltriethoxysilane (KH550), fumed silica and light calcium carbonate filler to obtain component B.

[0080] (3) Component A and component B are mixed in a weight ratio of 1:0.5, and stirred until the mixture is uniformly mixed to obtain the desired halogen-free flame-retardant low-density polyurethane sealant.

[0081] Comparative Example 2

[0082] This comparative example provides a commercially available halogen-free flame-retardant low-density polyurethane sealant, which is composed of component A and component B in a weight ratio of 1.5:0.5. The raw materials of component A in weight ratio include: 44 parts of polyol with a molecular weight of 500, 4 parts of dibutyl sebacate, 10 parts of terminal hydroxyl polybutadiene, 10 parts of ethylene glycol, 0.2 parts of dibutyl tin dilaurate, 2 parts of fumed silica, 1 part of fluorosilicone, 3 parts of r-glycidoxypropyltrimethylsilane (KH560), and 10 parts of light calcium carbonate.

[0083] The raw materials of the B component include, by weight, 15 parts of diphenylmethane diisocyanate (MDI), 2 parts of r-aminopropyltriethoxysilane (KH550), 2 parts of fumed silica, and 10 parts of light calcium carbonate.

[0084] This comparative example also provides a preparation method of the above-mentioned halogen-free flame-retardant low-density polyurethane sealant, which is as follows: (1) Preparation of component A: The polyol with a molecular weight of 500 and light calcium carbonate are stirred evenly, and then dehydrated at a high temperature of 110°C for 5 hours; the temperature is lowered to below 80°C, and dibutyl sebacate, terminal hydroxy polybutadiene, ethylene glycol, dibutyl tin dilaurate, fumed silica, fluorosilicone, and r-glycidoxypropyltrimethylsilane (KH560) are added at once, and stirred evenly to obtain component A.

[0085] (2) Preparation of component B: Dehydrate the light calcium carbonate filler at a high temperature of 110°C for 5 hours; stir and mix phenylmethane diisocyanate (MDI), r-aminopropyltriethoxysilane (KH550), fumed silica and light calcium carbonate filler to obtain component B.

[0086] (3) Component A and component B are mixed in a weight ratio of 1:0.5, and stirred until the mixture is uniformly mixed to obtain the desired halogen-free flame-retardant low-density polyurethane sealant.

[0087] The halogen-free flame-retardant low-density polyurethane sealants prepared in the above embodiments and comparative examples were tested. The test methods adopted were all conventional, such as the tensile property test method according to GB / T 2568-1995 and the oxygen index test method according to GB / T8294-2005. The specific test results are shown in Table 1.

[0088] Table 1

[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A halogen-free flame-retardant low-density polyurethane sealant, comprising component A and component B, characterized in that: The component A comprises the following raw materials in weight ratio: 60-90 parts of modified polyether polyol; 2-10 parts of plasticizer, 10-25 parts of toughening agent, 10-20 parts of chain extender, 0.1-0.5 parts of catalyst, 1-5 parts of thickener, 0.5-1.5 parts of defoamer, 1-5 parts of coupling agent, 10-30 parts of filler, 5-30 parts of flame retardant; the modified polyether polyol is composed of biopolyol and polyether polyol in a dosage ratio of 1:1-1.5; The B component comprises the following raw materials in weight ratio: 10-20 parts of polyisocyanate, 1-5 parts of coupling agent, 1-5 parts of thickener, 10-30 parts of filler and 10-30 parts of flame retardant.

2. The halogen-free flame-retardant low-density polyurethane sealant according to claim 1, characterized in that: The weight ratio of the component A to the component B is (1-1.5):0.5; preferably (1-1.2):0.

5.

3. The halogen-free flame-retardant low-density polyurethane sealant according to claim 1 or 2, characterized in that: The biopolyol is one or a combination of castor oil, modified castor oil, soybean oil, and palm oil; and / or the polyether polyol is one or a combination of polyether polyols with a functionality of 2 or 3 and polyether polyols with a molecular weight of 500-3000.

4. The halogen-free flame-retardant low-density polyurethane sealant according to any one of claims 1 to 3, characterized in that: The plasticizer is one or a combination of diisononyl phthalate, dibutyl phthalate, acetylcitrate tributyl dioctyl dicarboxylate, triphenyl phosphate, dibutyl sebacate, and dioctyl sebacate; and / or the toughening agent is hydroxyl-terminated polybutadiene or hydroxyl-terminated butadiene cyanide rubber.

5. The halogen-free flame-retardant low-density polyurethane sealant according to any one of claims 1 to 4, characterized in that: The chain extender is selected from 1,4-butanediol, ethylene glycol, 1,6-hexanediol, pentanediol, trimethylolpropane, hydroquinone dihydroxyethyl ether, resorcinol dihydroxyethyl ether, di-o-chlorodiphenylamine, dimethylthiotoluenediamine, 2,4-diamino-3,5-dimethylthiochlorobenzene, 2,4-diamino-5-mercaptotoluene, 4,4'-methylene-bis(3-chloro-2,6-diethylaniline, 4,4'-diaminodiphenylmethane, or a combination thereof; and / or the catalyst is selected from stannous octoate, dioctyltin dilaurate, dimethyltin dilaurate, dibutyltin dilaurate, butyltin oxide, octyltin oxide and triethanolamine, or a combination thereof.

6. The halogen-free flame-retardant low-density polyurethane sealant according to any one of claims 1 to 5, characterized in that: The thickener is one selected from fumed silica, hydrogenated castor oil and hydrated aluminum silicate; and / or the defoamer is at least one selected from polydimethylsiloxane, fluorosilicone and ethylene glycol siloxane.

7. The halogen-free flame-retardant low-density polyurethane sealant according to any one of claims 1 to 6, characterized in that: The coupling agent is selected from one or a combination of r-methacryloxypropyltrimethoxysilane (KH570), r-glycidoxypropyltrimethoxysilane (KH560), r-aminopropyltriethoxysilane (KH550); and / or the filler is selected from one or a combination of organic modified bentonite, hollow glass microspheres, hollow phenolic resin, ceramic hollow microspheres, pulverized coal hollow microspheres, hollow carbon microspheres and one or a combination of nano-scale light calcium carbonate, nano-talc powder, nano-silicon powder, nano-titanium dioxide.

8. The halogen-free flame-retardant low-density polyurethane sealant according to any one of claims 1 to 7, characterized in that: The flame retardant is a mixture of liquid flame retardant and powder flame retardant, and is selected from a combination of two or more of nano-aluminum hydroxide, nano-strong magnesium oxide, nano-ammonium polyphosphate, nano-melamine cyanurate, ammonium polyphosphate, trimethyl phosphate, trioctyl phosphate, and diphenyl ethyl hexyl phosphate.

9. The halogen-free flame-retardant low-density polyurethane sealant according to any one of claims 1 to 8, characterized in that: The isocyanate is selected from toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, 1,6-adipic acid diisocyanate, 1-isocyanate-3-isocyanatomethyl-3,5,5-trimethylcyclohexane (isophoron diisocyanate and 4,4'-diisocyanate dicyclohexylmethane, or a combination of several thereof.

10. The method for preparing the halogen-free flame-retardant low-density polyurethane sealant according to any one of claims 1 to 9, characterized in that: include: (1) mixing biopolyol and polyether polyol in a ratio of 1:1-1.5 to obtain modified polyether polyol; The modified polyether polyol, filler and powder flame retardant are mixed evenly, and then dehydrated at 100-115°C for 4-6 hours. After cooling to below 80°C, plasticizer, toughening agent, chain extender, catalyst, thickener, defoamer, coupling agent and liquid flame retardant are added and mixed evenly to obtain component A. (2) Stir the filler and powder flame retardant and dehydrate them at a high temperature of 100-115°C for 4-6 hours; mix the isocyanate, coupling agent, thickener, filler and flame retardant, stir and mix them evenly to obtain component B.

Citation Information

Patent Citations

  • Flame-retardant polyurethane sealant and preparation method thereof

    CN115074073A

  • Heat-resistant polyurethane sealant and preparation method thereof

    CN117025160A

Cited By

  • Low-density low-thermal-conductivity two-component polyurethane structural adhesive and preparation method thereof

    CN119463787A