Preparation of resin-coated nano calcium carbonate and application of resin-coated nano calcium carbonate in water-based drilling fluid

By coating the surface of nano calcium carbonate, the problem of poor agglomeration and dispersion capabilities in water-based drilling fluid is solved, the sealing performance and pressure bearing capacity are improved, and it is suitable for shale gas development and more efficient well wall stability and formation pressure.

CN118909604AInactive Publication Date: 2024-11-08SOUTHWEST PETROLEUM UNIV

Patent Information

Application Number
CN202411413171.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Simple nano calcium carbonate is prone to agglomeration in water-based drilling fluid and has poor dispersion capabilities, resulting in insufficient sealing performance and pressure bearing capacity, making it difficult to effectively seal micro-nano-scale cracks and pores in shale gas formations.

Method used

By coating the surface of nano calcium carbonate with high toughness resin, a high toughness resin coated with nano calcium carbonate is prepared to improve its dispersion and stability in water-based drilling fluid, and enhance the sealing performance and pressure bearing capacity. The method includes precipitating nano calcium carbonate at room temperature, reacting with resin monomer after modification, forming a high toughness resin coating, and obtaining a nanosealing agent by centrifugation and drying.

Benefits of technology

Improve the dispersion and sealing performance of nano calcium carbonate, enhance the pressure bearing capacity of water-based drilling fluid, significantly reduce the filtration loss of drilling fluid, improve the stability of the well wall and the formation pressure bearing capacity, and is suitable for shale gas etc. The development of unconventional natural gas resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the field of oilfield chemistry, and discloses preparation of resin-coated nano calcium carbonate and application of the resin-coated nano calcium carbonate in water-based drilling fluid, especially application of the resin-coated nano calcium carbonate as a nano plugging agent. The method comprises the following steps: firstly, preparing nano calcium carbonate by a precipitation method, and carrying out surface modification to enhance the compatibility of the nano calcium carbonate and resin; and then, coating the surface of the nano calcium carbonate with high-toughness resin by initiating a polymerization reaction to form the plugging material with high strength and excellent toughness. The prepared nano plugging agent shows excellent dispersity in water-based drilling fluid, can effectively plug well wall cracks and micropores, remarkably improves the stability and plugging effect of the drilling fluid, and is particularly suitable for drilling operation of complex stratums such as deep wells / ultra-deep wells and unconventional shale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This patent invention relates to the field of oilfield chemistry, specifically to the preparation of resin-coated nano-calcium carbonate and its application in water-based drilling fluid. Background Art

[0002] With the continuous growth of global energy demand, the development of unconventional natural gas resources such as shale gas has gradually become a key research direction in the energy field. However, shale gas reservoirs usually have complex geological characteristics, such as the development of a large number of micro-nanoscale cracks and pores. These characteristics can easily lead to problems such as wellbore instability and well leakage during drilling, seriously affecting the safety and efficiency of drilling operations. In order to effectively solve these problems, the performance requirements of drilling fluids are increasing, especially in complex formation conditions such as deep wells, ultra-deep wells, high temperature and high pressure, which puts higher requirements on the plugging performance, rheology, and pressure bearing capacity of drilling fluids.

[0003] Traditional oil-based drilling fluids are widely used in shale gas drilling due to their excellent plugging and lubrication properties, but their poor environmental performance and high cost limit their widespread promotion and application. In recent years, water-based drilling fluids have gradually become a research hotspot due to their environmental performance and low cost. However, the application of water-based drilling fluids in shale gas formations faces significant challenges, especially how to effectively plug micro-nanoscale cracks and pores to prevent wellbore instability and drilling fluid loss problems, while ensuring high pressure bearing capacity in complex formations.

[0004] Nano calcium carbonate has shown good application prospects as a nano plugging agent for water-based drilling fluids due to its small particle size and large specific surface area. However, pure nano calcium carbonate is easy to agglomerate in water-based drilling fluids, resulting in poor dispersibility, which in turn affects the plugging effect. To this end, by coating a layer of high-toughness resin on the surface of nano calcium carbonate, its dispersibility and stability in the drilling fluid can be effectively improved, and its plugging performance and pressure bearing capacity can be enhanced. High-toughness resin-coated nano calcium carbonate can not only improve the mechanical strength of the nano plugging agent, but also remain stable under high pressure conditions, effectively plugging cracks and pores in the well wall, significantly reducing the loss of drilling fluid, and enhancing the pressure bearing capacity of the formation, thereby improving the safety and efficiency of drilling operations.

[0005] The present invention proposes a method for preparing high-toughness resin-coated nano calcium carbonate, and studies its application in water-based drilling fluid. The high-toughness resin-coated nano calcium carbonate prepared by this method can be evenly dispersed in the water-based drilling fluid, which not only significantly improves its plugging performance, but also greatly improves the pressure bearing capacity of the drilling fluid, and is suitable for the efficient development of unconventional natural gas resources such as shale gas. Summary of the invention

[0006] The purpose of this patent invention is to overcome the problems of simple nano-calcium carbonate being easy to agglomerate and having poor dispersion ability in water-based drilling fluid, and to provide a preparation method of high-toughness resin-coated nano-calcium carbonate and its application in water-based drilling fluid.

[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for preparing high-toughness resin-coated nano calcium carbonate, the method comprising: (1) Under room temperature, the sodium carbonate solution is stirred at a certain speed, the calcium chloride solution is added to the sodium carbonate solution at a certain drop speed, and the mixture is stirred for a certain period of time, and then separated by a centrifuge to obtain nano calcium carbonate precipitate; (2) slowly adding the nano-calcium carbonate precipitate into a sodium dodecyl sulfate solution at room temperature and stirring, separating the modified nano-calcium carbonate again by centrifugation, and washing twice with ethanol to obtain modified nano-calcium carbonate; (3) dispersing the modified nano-calcium carbonate in anhydrous ethanol in a certain proportion, adding the resin monomer, adding the initiator, maintaining the stirring speed of the solution, and raising the reaction temperature for a certain reaction time to obtain a high-toughness resin-coated nano-calcium carbonate solution; (4) The high-toughness resin-coated nano-calcium carbonate solution is centrifuged, the particles are repeatedly washed with anhydrous ethanol for three times, and then dried in a vacuum drying oven to obtain a high-toughness resin-coated nano-calcium carbonate nano plugging agent.

[0008] The second aspect of the present invention provides a high-toughness resin-coated nano calcium carbonate prepared by the method described in the first aspect.

[0009] The third aspect of the present invention provides the use of the high-toughness resin-coated nano-calcium carbonate described in the second aspect as a nano-plugging agent in water-based drilling fluid.

[0010] Through the above technical solution, the present invention can achieve the following beneficial effects: (1) The high-toughness resin-coated nano calcium carbonate prepared by the method provided by the invention of this patent has good hydrophilicity, and the initial particle size of the nano calcium carbonate is 20-100 nanometers; the thickness of the high-toughness resin coating layer is 5-50 nanometers, and it is not easy to agglomerate in water-based drilling fluid, has good dispersion effect, and has strong pressure bearing capacity. It can effectively block the nano-scale pores in the shale formation, delay the transmission of pore pressure, and improve the pressure bearing capacity of the formation; (2) The water-based drilling fluid provided by the present invention contains the aforementioned high-toughness resin-coated nano-calcium carbonate. The water-based drilling fluid has good rheological properties, high plugging rate, strong adaptability, can greatly improve the wellbore stability, and is beneficial to reservoir protection. DETAILED DESCRIPTION

[0011] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0012] The specific implementation of the present invention is described in detail below. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0013] The first aspect of the present invention provides a method for preparing high-toughness resin-coated nano calcium carbonate, the method comprising: (1) Under room temperature, the sodium carbonate solution is stirred at a certain speed, the calcium chloride solution is added to the sodium carbonate solution at a certain drop speed, and the mixture is stirred for a certain period of time, and then separated by a centrifuge to obtain nano calcium carbonate precipitate; (2) slowly adding the nano-calcium carbonate precipitate into a sodium dodecyl sulfate solution at room temperature and stirring, separating the modified nano-calcium carbonate again by centrifugation, and washing twice with ethanol to obtain modified nano-calcium carbonate; (3) dispersing the modified nano-calcium carbonate in anhydrous ethanol in a certain proportion, adding the resin monomer, adding the initiator, maintaining the stirring speed of the solution, and raising the reaction temperature for a certain reaction time to obtain a high-toughness resin-coated nano-calcium carbonate solution; (4) The high-toughness resin-coated nano-calcium carbonate solution is centrifuged, the particles are repeatedly washed with anhydrous ethanol for three times, and then dried in a vacuum drying oven to obtain a high-toughness resin-coated nano-calcium carbonate nano plugging agent.

[0014] According to the invention of this patent, in step (1), at room temperature, the sodium carbonate solution is kept at a certain stirring speed, the calcium chloride solution is added to the sodium carbonate solution at a certain dropwise acceleration, and after continuous stirring for a certain period of time, a centrifuge is used to separate and obtain nano calcium carbonate precipitate.

[0015] According to the invention of this patent, in step (1), the mass concentration of the sodium carbonate solution is 52.995 g / L, and the mass concentration of the calcium chloride solution is 55.49 g / L.

[0016] According to the invention of this patent, in step (1), the weight ratio of the sodium carbonate solution to the calcium chloride solution is 100: (90-130), preferably 1: (100-120); According to the invention of this patent, in step (1), the reaction conditions include: reaction temperature is room temperature; dropwise addition speed is 1-3 mL / min; stirring speed is 200-400 rpm; stirring time is 50-70 min; centrifuge speed is 4000-6000 rpm, and centrifugation time is 10-20 min; According to the invention of this patent, in step (1), after the reaction is completed, the nano calcium carbonate precipitate is obtained.

[0017] In this patent invention, room temperature refers to 20-25°C.

[0018] According to the invention of this patent, in step (2), the nano calcium carbonate precipitate is slowly added to the sodium dodecyl sulfate solution at room temperature and stirred, and the modified nano calcium carbonate is separated again by centrifugation, and washed twice with ethanol to obtain modified nano calcium carbonate; According to the invention of this patent, in step (2), preferably, the weight ratio of the nano calcium carbonate precipitate: sodium dodecyl sulfate solution is 1: (8-12), preferably 1: (9-11); the mass concentration of the sodium dodecyl sulfate solution is 2%; According to the invention of this patent, in step (2), the reaction conditions include: reaction temperature is room temperature; stirring time is 1-3 h; stirring speed is 200-400 rpm; centrifuge speed is 4000-6000 rpm, and centrifugation time is 10-20 min; According to the invention of this patent, in step (2), after the reaction is completed, the modified nano calcium carbonate is obtained.

[0019] According to the invention of this patent, in step (3), the modified nano-calcium carbonate is dispersed in anhydrous ethanol in a certain proportion, and after adding the resin monomer, an initiator is added, the stirring speed of the solution is maintained, and the reaction temperature is increased for a certain reaction time to obtain a nano-calcium carbonate solution coated with a high-toughness resin; According to the invention of this patent, in step (3), the resin monomer is selected from one of ethyl acrylate, acrylic acid, acrylamide and methyl methacrylate, preferably methyl methacrylate; According to the invention of this patent, in step (3), the initiator is selected from one of azobisisobutyronitrile, benzoyl peroxide, azobisisoheptanenitrile and ammonium persulfate, preferably ammonium persulfate; According to the invention of this patent, in step (3), the weight ratio of the modified nano-calcium carbonate: anhydrous ethanol: resin monomer: initiator is 100: (180-220): (180-220): (1-3), preferably 100: (190-210): (190-210): (1.5-2.5).

[0020] The second aspect of the present invention provides that the initial particle size of the nano calcium carbonate prepared by the method described in the first aspect is 20-100 nm, preferably 40-80 nm; According to the invention of this patent, in step (3), the reaction conditions include: reaction temperature of 60-70 °C; stirring speed of 200-400 rpm; reaction time of 2-4 h.

[0021] The second aspect of the present invention provides a high-toughness resin coating layer of high-toughness resin-coated nano-calcium carbonate prepared by the method described in the first aspect, the thickness of which is 5-50 nm, preferably 10-30 nm.

[0022] According to the invention of this patent, the high-toughness resin-coated nano calcium carbonate has strong hydrophilicity, can be well dispersed in the water phase, is not easy to agglomerate in the water-based drilling fluid system, has a good dispersion effect, and can obtain excellent plugging effect at a lower concentration, thereby reducing the formation permeability and preventing the intrusion of drilling fluid.

[0023] According to the invention of this patent, the high-toughness resin-coated nano calcium carbonate has a strong pressure-bearing capacity, can delay the transmission of pore pressure in the formation, and improve the pressure-bearing capacity of the formation.

[0024] According to the invention of this patent, the high-toughness resin-coated nano-calcium carbonate has little effect on the viscosity and shear force of the water-based drilling fluid, has good compatibility and strong adaptability.

[0025] The third aspect of the present invention provides the use of the high-toughness resin-coated nano-calcium carbonate described in the second aspect as a nano-plugging agent in water-based drilling fluid.

[0026] The fourth aspect of the present invention provides a water-based drilling fluid, which contains the high-toughness resin-coated nano-calcium carbonate described in the second aspect.

[0027] According to the invention of this patent, the water-based drilling fluid includes the following components: 100 parts by weight of base fluid, 7-13 parts by weight of bentonite, 0.6-1.4 parts by weight of polymer viscosity enhancer, 3-9 parts by weight of fluid loss reducer, 3-7 parts by weight of conventional plugging agent, 1-5 parts by weight of lubricant, 4-8 parts by weight of inhibitor, 1.5-2.5 parts by weight of pH adjuster, 0.5-1.5 parts by weight of nano plugging agent, and 80-300 parts by weight of weighting agent.

[0028] According to the invention of this patent, on the basis of satisfying the above-mentioned composition, preferably, the water-based drilling fluid includes the following components: 100 parts by weight of base fluid, 9-11 parts by weight of bentonite, 0.8-1.2 parts by weight of polymer viscosity enhancer, 5-7 parts by weight of fluid loss reducer, 4-6 parts by weight of conventional plugging agent, 2-4 parts by weight of lubricant, 5-6 parts by weight of inhibitor, 1.8-2.2 parts by weight of pH adjuster, 0.8-1.2 parts by weight of nano plugging agent, and 150-250 parts by weight of weighting agent.

[0029] According to the invention of this patent, the base liquid is tap water, and the invention of this patent has no special limitation on this.

[0030] According to the present invention, the bentonite is at least one of sodium-based bentonite, calcium-based bentonite and calcium-sodium-based bentonite, and more preferably sodium-based bentonite. In the present invention, the sodium-based bentonite can be obtained by self-production using conventional methods in the art, or it can be a conventional commercially available product, and the present invention has no particular limitation on this.

[0031] According to the invention of this patent, the polymer thickener is selected from at least carboxymethyl cellulose, polyanionic cellulose, magnetic polyacrylamide and guar gum, and is more preferably carboxymethyl cellulose. The carboxymethyl cellulose can be divided into low-viscosity carboxymethyl cellulose (viscosity range: 10-200 mPa·s), medium-viscosity carboxymethyl cellulose (viscosity range: 200-1500 mPa·s), and high-viscosity carboxymethyl cellulose (viscosity range: 1500-5000 mPa·s) according to viscosity, and is more preferably medium-viscosity carboxymethyl cellulose.

[0032] According to the invention of this patent, the fluid loss reducer is selected from at least carboxymethyl starch, sulfonated lignin, acrylamide / sodium acrylate copolymer and polyvinyl alcohol, and carboxymethyl starch is more preferably used. The carboxymethyl starch can be divided into low-substituted carboxymethyl starch (substitution degree: 0.1-0.3), medium-substituted carboxymethyl starch (substitution degree: 0.3-0.5), and high-substituted carboxymethyl starch (substitution degree: above 0.5) according to the degree of substitution, and high-substituted carboxymethyl starch is more preferably used.

[0033] According to the invention of this patent, the conventional plugging agent is selected from one of fine-grained limestone, cellulose fiber and modified paraffin, and is further preferably fine-grained limestone.

[0034] According to the invention of this patent, the weighting agent can be a conventional weighting agent for drilling fluid in the art. Preferably, the weighting agent is selected from at least one of API barite, ultrafine barium sulfate, magnetite powder, ilmenite powder and manganese tetraoxide, and more preferably API barite.

[0035] The water-based drilling fluid system provided by this patent invention effectively seals formation cracks and micropores, prevents hydration and expansion of clay minerals in the formation after reacting with water, helps to enhance well wall stability and reduce the risk of well wall collapse; effectively controls drilling fluid filtration loss, prevents mud filtrate from entering the formation, and protects the reservoir; helps to carry drill cuttings, improve drilling efficiency, and ensure well bottom cleanliness; these advantages make the water-based drilling fluid have excellent performance in shale gas drilling, can effectively cope with complex formation environments, and improve drilling efficiency and operation safety.

[0036] The invention of this patent will be described in detail below through examples. In the following preparation examples, examples and comparative examples; Base fluid: tap water; Bentonite: sodium bentonite, purchased from Qingdao Runtu Bentonite Co., Ltd.; Polymer thickener: medium viscosity carboxymethyl cellulose, purchased from Qingdao Runtu Bentonite Co., Ltd.; Fluid loss reducer: carboxymethyl starch, purchased from Hebei Yanxing Chemical Co., Ltd.; Conventional plugging agent: fine-grained limestone, purchased from Sichuan Southwest Shida Technology Co., Ltd.; Commercially available nano plugging agent: nano calcium carbonate, purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.; Unless otherwise specified, other materials used are common commercially available products.

[0037] Preparation Example 1 (Preparation Example 1 uses preferred raw materials and conditions to prepare a preferred high-toughness resin-coated nano-calcium carbonate product) (1) At room temperature, 110 parts by weight of calcium chloride solution was slowly added dropwise to 100 parts by weight of sodium carbonate solution, the stirring speed was maintained at 300 rpm, the dropping speed was maintained at 2·mL / min; and the stirring was continued for 60 min to generate nano calcium carbonate precipitate. After the reaction was completed, the precipitate was separated by centrifugation (5000 rpm, 15 min), and was repeatedly washed with deionized water for 3 times to obtain nano calcium carbonate precipitate; (2) At room temperature, 100 parts by weight of the nano-calcium carbonate precipitate was redispersed in a sodium dodecyl sulfate solution (mass concentration of 2%), the solution was stirred at a speed of 300 rpm for 2 h, and the modified nano-calcium carbonate was separated again by centrifugation (5000 rpm, 15 min), and washed twice with ethanol to obtain modified nano-calcium carbonate; (3) dispersing 100 parts by weight of modified nano-calcium carbonate in 200 parts by weight of anhydrous ethanol, adding 200 parts by weight of methyl methacrylate, adding 2 parts by weight of ammonium persulfate, maintaining the stirring speed of the solution at 300 rpm, the reaction temperature at 65°C, and the reaction time at 3 h to obtain a high-toughness resin-coated nano-calcium carbonate solution; (4) The high-toughness resin-coated nano-calcium carbonate solution was separated by centrifugation (5000 rpm, 15 min), and the particles were repeatedly washed with anhydrous ethanol for 3 times. The washed nano-calcium carbonate particles were dried in a vacuum drying oven at 60°C for 24 h to obtain the final high-toughness resin-coated nano-calcium carbonate nano-plugging agent (denoted as S1).

[0038] Preparation Example 2 (Preparation Example 2 uses preferred raw materials and conditions to prepare a preferred high-toughness resin-coated nano-calcium carbonate product) (1) At room temperature, 100 parts by weight of calcium chloride solution was slowly added dropwise to 100 parts by weight of sodium carbonate solution, the stirring speed was maintained at 300 rpm, the dropping speed was maintained at 2 mL / min, and the stirring was continued for 60 min to generate nano calcium carbonate precipitate. After the reaction was completed, the precipitate was separated by centrifugation (5000 rpm, 15 min), and was repeatedly washed with deionized water for 3 times to obtain nano calcium carbonate precipitate. (2) At room temperature, 100 parts by weight of the nano-calcium carbonate precipitate was redispersed in a sodium dodecyl sulfate solution (mass concentration of 2%), the solution was stirred at a speed of 300 rpm for 2 h, and the modified nano-calcium carbonate was separated again by centrifugation (5000 rpm, 15 min), and washed twice with ethanol to obtain modified nano-calcium carbonate; (3) dispersing 100 parts by weight of modified nano-calcium carbonate in 210 parts by weight of anhydrous ethanol, adding 210 parts by weight of methyl methacrylate, adding 2.5 parts by weight of ammonium persulfate, maintaining the stirring speed of the solution at 300 rpm, the reaction temperature at 65°C, and the reaction time at 3 h to obtain a high-toughness resin-coated nano-calcium carbonate solution; (4) The nano calcium carbonate solution coated with high toughness resin was separated by centrifugation (5000 rpm, 15 min), and the particles were repeatedly washed with anhydrous ethanol for 3 times. The washed nano calcium carbonate particles were dried in a vacuum drying oven at 60°C for 24 h to obtain the final nano plugging agent (denoted as S2).

[0039] Preparation Example 3 (Preparation Example 3 uses non-preferred raw materials and conditions to prepare a non-preferred high-toughness resin-coated nano-calcium carbonate product) (1) At room temperature, 80 parts by weight of calcium chloride solution was slowly added dropwise to 100 parts by weight of sodium carbonate solution, the stirring speed was maintained at 300 rpm, the dropping speed was maintained at 2·mL / min; and the stirring was continued for 60 min to generate nano calcium carbonate precipitate. After the reaction was completed, the precipitate was separated by centrifugation (5000 rpm, 15 min), and was repeatedly washed with deionized water for 3 times to obtain nano calcium carbonate precipitate; (2) At room temperature, 100 parts by weight of the nano-calcium carbonate precipitate was redispersed in a sodium dodecyl sulfate solution (mass concentration of 2%), the solution was stirred at a speed of 300 rpm for 2 h, and the modified nano-calcium carbonate was separated again by centrifugation (5000 rpm, 15 min), and washed twice with ethanol to obtain modified nano-calcium carbonate; (3) dispersing 100 parts by weight of modified nano-calcium carbonate in 170 parts by weight of anhydrous ethanol, adding 170 parts by weight of methyl methacrylate, adding 0.5 parts by weight of ammonium persulfate, maintaining the stirring speed of the solution at 300 rpm, the reaction temperature at 65°C, and the reaction time at 3 h to obtain a high-toughness resin-coated nano-calcium carbonate solution; (4) The high-toughness resin-coated nano-calcium carbonate solution was separated by centrifugation (5000 rpm, 15 min), and the particles were repeatedly washed with anhydrous ethanol for 3 times. The washed nano-calcium carbonate particles were dried in a vacuum drying oven at 60°C for 24 h to obtain the final high-toughness resin-coated nano-calcium carbonate nano-plugging agent (denoted as S3).

[0040] Example 1 (the dosage of each component of the drilling fluid in Example 1 adopts the lower limit of the preferred range in right 9) 100 parts by weight of tap water and 10 parts by weight of bentonite were stirred at a stirring rate of 1000 r / min for 60 minutes and then allowed to stand for 24 hours. Then, 1 part by weight of polymer viscosity enhancer was added and stirred at a stirring rate of 2000 r / min for 30 minutes. Then, 6 parts by weight of fluid loss reducer was added and stirred at a stirring rate of 2000 r / min for 20 minutes. Then, 5 parts by weight of conventional plugging agent was added and stirred at a stirring rate of 2000 r / min for 10 minutes. Then, 3 parts by weight of lubricant was added and stirred at a stirring rate of 1000 r / min. min and stirred for 10 min at a stirring rate of 2000 r / min, then 5.5 parts by weight of an inhibitor was added and stirred for 10 min at a stirring rate of 2000 r / min, then 2 parts by weight of a pH adjuster was added and stirred for 10 min at a stirring rate of 1000 r / min, then 1 part by weight of a nano plugging agent S1 was added and stirred for 30 min at a stirring rate of 2000 r / min, then 200 parts by weight of a weighting agent was added and stirred for 30 min at a stirring rate of 2000 r / min to obtain a water-based drilling fluid (denoted as F1).

[0041] The components and contents of F1 are shown in Table 1.

[0042] Example 2-3 The method of Example 1 is followed, except that S2 and S3 are used as nano plugging agents, respectively, and other conditions are the same as those of Example 1. Water-based drilling fluids (respectively denoted as F2 and F3) are obtained.

[0043] Example 4 (the dosage of each component of the drilling fluid in Example 4 adopts the upper limit of the preferred range in right 9) 100 parts by weight of tap water and 11 parts by weight of bentonite were stirred at a stirring rate of 1000 r / min for 60 min and then allowed to stand for 24 h. Then, 1.2 parts by weight of polymer thickener were added and stirred at a stirring rate of 2000 r / min for 30 min. Then, 7 parts by weight of fluid loss reducer were added and stirred at a stirring rate of 2000 r / min for 20 min. Then, 6 parts by weight of conventional plugging agent were added and stirred at a stirring rate of 2000 r / min for 10 min. Then, 4 parts by weight of lubricant were added and stirred at 1000 r / min. / min and stirred for 10 min at a stirring rate of 1000 r / min, then 6 parts by weight of an inhibitor was added and stirred for 10 min at a stirring rate of 2000 r / min, then 2.2 parts by weight of a pH adjuster was added and stirred for 10 min at a stirring rate of 1000 r / min, then 1.2 parts by weight of a nano plugging agent S1 was added and stirred for 30 min at a stirring rate of 2000 r / min, then 250 parts by weight of a weighting agent was added and stirred for 30 min at a stirring rate of 2000 r / min to obtain a water-based drilling fluid (denoted as F4).

[0044] The components and contents of F4 are shown in Table 1.

[0045] Embodiment 5-6 The method of Example 4 is followed, except that S2 and S3 are used as nano plugging agents, respectively, and other conditions are the same as those of Example 4. Water-based drilling fluids (respectively denoted as F5 and F6) are obtained.

[0046] Example 7 (the dosage of each component of the drilling fluid in Example 7 adopts the lower limit of the non-preferred range in Weight 9) 100 parts by weight of tap water and 7 parts by weight of bentonite were stirred at a stirring rate of 1000 r / min for 60 minutes and then allowed to stand for 24 hours. Then, 0.6 parts by weight of polymer viscosity enhancer was added and stirred at a stirring rate of 2000 r / min for 30 minutes. Then, 3 parts by weight of fluid loss reducer was added and stirred at a stirring rate of 2000 r / min for 20 minutes. Then, 3 parts by weight of conventional plugging agent was added and stirred at a stirring rate of 2000 r / min for 10 minutes. Then, 1 part by weight of lubricant was added and stirred at a stirring rate of 1000 r / min. min and stirred for 10 min at a stirring rate of 1000 r / min, then 4 parts by weight of an inhibitor was added and stirred for 10 min at a stirring rate of 2000 r / min, then 1.5 parts by weight of a pH adjuster was added and stirred for 10 min at a stirring rate of 1000 r / min, then 0.5 parts by weight of a nano plugging agent S1 was added and stirred for 30 min at a stirring rate of 2000 r / min, then 80 parts by weight of a weighting agent was added and stirred for 30 min at a stirring rate of 2000 r / min to obtain a water-based drilling fluid (denoted as F7).

[0047] The components and contents of F7 are shown in Table 1.

[0048] Embodiment 8-9 The method of Example 7 is followed, except that S2 and S3 are used as nano plugging agents, respectively, and other conditions are the same as those of Example 7. Water-based drilling fluids (respectively denoted as F8 and F9) are obtained.

[0049] Example 10 (the dosage of each component of the drilling fluid in Example 10 adopts the upper limit of the non-preferred range in Weight 9) 100 parts by weight of tap water and 13 parts by weight of bentonite were stirred at a stirring rate of 1000 r / min for 60 min and then allowed to stand for 24 h. Then 1.4 parts by weight of polymer viscosity enhancer were added and stirred at a stirring rate of 2000 r / min for 30 min. Then 9 parts by weight of fluid loss reducer were stirred at a stirring rate of 2000 r / min for 20 min. Then 7 parts by weight of conventional plugging agent were added and stirred at a stirring rate of 2000 r / min for 10 min. Then 5 parts by weight of lubricant were added and stirred at a stirring rate of 1000 r / min. min and stirred for 10 min at a stirring rate of 1000 r / min, then 8 parts by weight of an inhibitor was added and stirred for 10 min at a stirring rate of 2000 r / min, then 2.5 parts by weight of a pH adjuster was added and stirred for 10 min at a stirring rate of 1000 r / min, then 1.5 parts by weight of nano plugging agent S1 was added and stirred for 30 min at a stirring rate of 2000 r / min, then 300 parts by weight of a weighting agent was added and stirred for 30 min at a stirring rate of 2000 r / min to obtain a water-based drilling fluid (denoted as F10).

[0050] The components and contents of F10 are shown in Table 1.

[0051] Examples 11-12 The method of Example 10 is followed, except that S2 and S3 are used as nano plugging agents, respectively, and other conditions are the same as those of Example 10. Water-based drilling fluids (respectively denoted as F11 and F12) are obtained.

[0052] Comparative Example 1 The method of Example 1 is followed, except that the nano plugging agent S1 is not added, and other conditions are the same as those of Example 1. A water-based drilling fluid (denoted as DF1) is obtained.

[0053] Comparative Example 2 The method of Example 1 is followed, except that the modified nano calcium carbonate prepared in step (2) of Preparation Example 1 is used as the nano plugging agent, and other conditions are the same as those of Example 1. A water-based drilling fluid (denoted as DF2) is obtained.

[0054] Comparative Example 3 The method of Example 2 is followed, except that the modified nano calcium carbonate prepared in step (2) of Preparation Example 2 is used as the nano plugging agent, and other conditions are the same as those of Example 2. A water-based drilling fluid (denoted as DF3) is obtained.

[0055] Comparative Example 4 The method of Example 3 is followed, except that the modified nano calcium carbonate prepared in step (2) of Preparation Example 3 is used as the nano plugging agent, and other conditions are the same as those of Example 3. A water-based drilling fluid (denoted as DF4) is obtained.

[0056] Comparative Example 5 The method of Example 1 is followed, except that the nano calcium carbonate precipitate obtained in step (1) of Preparation Example 1 is used as the nano plugging agent, and other conditions are the same as those of Example 1. A water-based drilling fluid (denoted as DF5) is obtained.

[0057] Comparative Example 6 The method of Example 1 is followed, except that S1 is replaced by commercially available nano calcium carbonate, and other conditions are the same as those of Example 1. A water-based drilling fluid (denoted as DF6) is obtained.

[0058] Comparative Example 7 The method of Example 1 was followed, except that the amount of S1 added was adjusted to 3 parts by weight, and the other conditions were the same as those of Example 1. A water-based drilling fluid (denoted as DF7) was obtained.

[0059] Table 1 Table 1 Note: In Table 1, the modified nano-calcium carbonate used in DF2-DF4 is the modified nano-calcium carbonate prepared in step (2) of Preparation Examples 1-3 respectively.

[0060] Test Case The nano calcium carbonate precipitate, modified nano calcium carbonate and nano plugging agent prepared in Preparation Example 1 were subjected to particle size test and Zeta potential test to evaluate their particle size and dispersibility, and the water-based drilling fluids F1-F12 prepared in Examples 1-12 and the water-based drilling fluids DF1-DF7 prepared in Comparative Examples 1-7 were tested for plugging performance, pressure bearing performance and compatibility performance. In the following test examples, Apparent viscosity (AV, mPa•s), plastic viscosity (PV, mPa•s), and dynamic shear force (YP, Pa) were measured using a six-speed rotary viscometer according to the method specified in GB / T29170-2012; Medium pressure filtration loss (API, mL) is measured using a medium pressure filtration instrument according to the method specified in GB / T29170-2012; High temperature and high pressure filtration loss (HTHP, mL) is measured using a high temperature and high pressure filtration instrument according to the method specified in GB / T29170-2012; The manufacturer of the laser particle size analyzer is Malvern Instruments of the United Kingdom; The manufacturer of the Zeta potential analyzer is Brookhaven Instruments, USA, model Nano-Brook Omni; The manufacturer of the six-speed rotational viscometer is Stillbo Company, model ZNN-D6S; The manufacturer of the medium-pressure filter loss meter is Steele Platt Company, model SD4 / SD4A; The manufacturer of the high-temperature and high-pressure filtration tester is Kence Instruments, model KC-GS173.

[0061] 1. Particle size and contact angle Particle size test: Add the nano plugging agent S1 into deionized water, stir thoroughly, and use a laser particle size analyzer to measure the particle size of the nano plugging agent after it is dispersed in deionized water, and observe the degree of dispersion; The results are shown in Table 2; Contact angle test: 300 mg of nano plugging agents S1-S3 were weighed respectively, and made into sample slices using a tablet press, and the contact angle of distilled water on the surface of the slices was measured using a contact angle meter; The results are shown in Table 2; Table 2 It can be seen from Table 2 that the particle sizes of the nano calcium carbonate precipitate, modified nano calcium carbonate and nano plugging agent S1 obtained in Preparation Example 1 are in the range of 82-113 nm, and the absolute value of the Zeta potential of the nano plugging agent S1 in deionized water is greater than 30, which indicates that the nano plugging agent prepared by the present invention has excellent dispersibility in the aqueous phase and does not agglomerate, so that it can be dispersed in the aqueous phase in nanometer size, thereby meeting the requirements for plugging the micropores in the formation.

[0062] 2. Sealing performance The base slurry (tap water + 6% bentonite + 5% sodium carbonate + 5% SMC-Ⅰ + 10% SMC-Ⅱ + 10% nanobarite, where the percentage of each component is based on the weight of tap water) was placed in a high-temperature and high-pressure filter loss instrument, and the high-temperature and high-pressure filter loss test was carried out for 60 min at 105°C and a pressure difference of 3.5 MPa. After the test, it was cooled to room temperature, the base slurry in the mud cup was poured out, and the filter cake was left at the bottom of the mud cup; deionized water was injected along the inner wall of the mud cup 1-2 times and gently shaken during the injection process, and then the deionized water was poured out to wash away the virtual mud on the filter cake; deionized water was injected into the mud cup to the scale, and the temperature was 105°C and the pressure difference was 3.5 MPa, the above high temperature and high pressure filtration loss test process was repeated for 30 min to further wash away the false mud. After the test, the mud was cooled to room temperature, deionized water was poured out, and the mud cake in the mud cup was taken out. The permeability of the mud cake of the base mud was calculated by formula (I) to be 3.852×10 -4 mD; using the above-mentioned base slurry mud cake as a simulated formation with micro-nano fractures; Where, K0: permeability, mD; q: average filtration loss per unit time, cm 3 / s; l: mud cake thickness, mm; μ: drilling fluid viscosity, mPa·s; A: mud cake area, m 2 ; ΔP: pressure difference, MPa; Drilling fluids F1-F12 and DF1-DF7 were used as test slurries for aging treatment (aging temperature was 105°C, aging time was 16 h), and after cooling to room temperature, they were placed in the mud cups of the high-temperature and high-pressure filter loss instrument (the base slurry cake at the bottom of the mud cup was used as the percolation medium), and the high-temperature and high-pressure filter loss test was carried out for 30 minutes at a temperature of 105°C and a pressure difference of 3.5 MPa. After the test, they were cooled to room temperature, the slurry in the mud cup was poured out, and the test slurry cake was left at the bottom of the mud cup; deionized water was injected along the inner wall of the mud cup 1-2 times and gently shaken during the injection process, and then the deionized water was poured out to wash away the virtual mud on the filter cake; deionized water was injected into the mud cup to the scale, and the above high-temperature and high-pressure filter loss test process was repeated at a temperature of 105°C and a pressure difference of 3.5 MPa for 30 minutes. min to further wash away the false mud. After the test, cool to room temperature, pour out the deionized water, take out the test slurry mud cake in the mud cup, and calculate the mud cake permeability (denoted as K1, mD) of the test slurries F1-F12 and DF1-DF7 according to the above formula (I). On this basis, the permeability reduction rate of the test slurries F1-F12 and DF1-DF7 before and after plugging the simulated formation is calculated using formula (II) (that is, the permeability reduction rate is used to characterize the plugging effect. The higher the permeability reduction rate, the better the plugging effect of the plugging material). The results are shown in Table 3. Among them, K r : Permeability reduction rate, %; K0: permeability of base mud cake (simulated formation), mD; K1: permeability of water-based drilling fluid mud cake, mD; Table 3 As can be seen from Table 3, through simulation tests, water-based drilling fluids F1-F12 use the high-toughness resin-coated nano calcium carbonate provided by the invention of this patent as a nano plugging agent, which can effectively plug the micro-nano cracks in the simulated formation, showing excellent plugging performance, and the permeability reduction rate is greater than 96%. However, water-based drilling fluid DF1 does not use nano plugging agents, the nano plugging agents used by DF2-DF4 are nano plugging agents that are not prepared according to the method of the invention of this patent, and DF5-DF6 use conventional commercial nano plugging agents or uncoated nano calcium carbonate as nano plugging agents, and the plugging effects are significantly worse than F1-F12. The excellent plugging performance obtained by F1-F12 is due to the fact that the high-toughness resin-coated nano calcium carbonate nano plugging agent used has good hydrophilicity, can be evenly dispersed in the water-based drilling fluid system, and has a suitable size and good pressure-bearing performance, thereby effectively plugging micro-nano cracks, reducing the formation permeability, and preventing the drilling fluid from invading the formation. In particular, DF7 does not adopt the water-based drilling fluid formula of the present application, and its plugging performance is somewhat inferior to that of F1-F12.

[0063] 3. Pressure bearing performance The 3D printed core was loaded into the formation micro-fracture plugging and pressure bearing capacity evaluation device, and the drilling fluids F1-F12 and DF1-DF7 were added to the device at 120°C, starting from 0MPa, with a gradient of 0.5MPa, and the pressure was maintained for 3 minutes each time until the pressure was increased to 6MPa and maintained for 3 minutes. During this process, the amount of drilling fluid (i.e., the amount of filtrate) driven out at different pressures is shown in Table 4; Table 4 As can be seen from Table 4, in the test of micro-fracture plugging and pressure bearing capacity evaluation of the formation, the water-based drilling fluid F1-F12 can withstand a pressure of 30 MPa, showing excellent pressure bearing performance, which is conducive to delaying the transmission of pore pressure and improving the pressure bearing capacity of the formation. In contrast, the pressure bearing performance of DF1-DF7 is poor.

[0064] 4. Compatibility Prepare water-based drilling fluid A (tap water + 10% bentonite + 1% polymer viscosity enhancer + 6% fluid loss reducer + 5% conventional plugging agent + 2.5% lubricant + 6% inhibitor + 2% pH adjuster, wherein the percentage of each component is based on the weight of tap water), then add 1% (based on the weight of tap water in the water-based drilling fluid A) of the high-toughness resin-coated nano-calcium carbonate S1 prepared in Preparation Example 1 to the water-based drilling fluid A to prepare water-based drilling fluid B; Table 5 It can be seen from Table 5 that the addition of the high-toughness resin-coated nano calcium carbonate S1 of the present invention has little effect on the rheological properties of the water-based drilling fluid, and the rheological properties are good, indicating that the high-toughness resin-coated nano calcium carbonate provided by the present invention has good compatibility as a nano plugging agent for water-based drilling fluid.

[0065] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a high-toughness resin-coated nano-calcium carbonate nano-plugging agent for water-based drilling fluid, It is characterized in that The following steps are involved: (1) At room temperature, the sodium carbonate solution is stirred at a speed of 200-400 rpm, and the calcium chloride solution is added dropwise to the sodium carbonate solution at a dropping speed of 1-3 mL / min, and the stirring is continued for 50-70 minutes, and then separated by a centrifuge to obtain nano calcium carbonate precipitate; (2) slowly adding the nano-calcium carbonate precipitate into a sodium dodecyl sulfate solution at room temperature and stirring, separating the modified nano-calcium carbonate again by centrifugation, and washing twice with ethanol to obtain modified nano-calcium carbonate; (3) dispersing the modified nano-calcium carbonate in anhydrous ethanol, adding a resin monomer, and then adding an initiator, maintaining the stirring speed of the solution, and increasing the reaction temperature to obtain a nano-calcium carbonate solution coated with a high-toughness resin; (4) The high-toughness resin-coated nano-calcium carbonate solution is centrifuged, the particles are repeatedly washed with anhydrous ethanol for three times, and then dried in a vacuum drying oven to obtain a high-toughness resin-coated nano-calcium carbonate nano plugging agent.

2. The method according to claim 1, in, In step (1), the weight ratio of the sodium carbonate solution to the calcium chloride solution is 100:(90-130).

3. The method according to claim 1, in, In step (2), the weight ratio of the nano-calcium carbonate precipitate to the sodium dodecyl sulfate solution is 1:(8-12); the mass concentration of the sodium dodecyl sulfate solution is 2%.

4. The method according to claim 1, in, In step (3), the weight ratio of the modified nano-calcium carbonate: anhydrous ethanol: resin monomer: initiator is 100: (180-220): (180-220): (1-3).

5. The method according to claim 1, in, In step (3): The resin monomer is selected from one of ethyl acrylate, acrylic acid, acrylamide and methyl methacrylate; The initiator is selected from one of azobisisobutyronitrile, benzoyl peroxide, azobisisoheptanenitrile and ammonium persulfate.

6. The method according to claim 1, in: In step (1), the reaction conditions include: the reaction temperature is room temperature; the centrifuge speed is 4000-6000 rpm, and the centrifugation time is 10-20 min; In step (2), the reaction conditions include: reaction temperature is room temperature; stirring time is 1-3 h; stirring speed is 200-400 rpm; centrifuge speed is 4000-6000 rpm, and centrifugation time is 10-20 min; In step (3), the reaction conditions include: reaction temperature of 60-70°C; stirring speed of 200-400 rpm; reaction time of 2-4 h; In step (4), the reaction conditions include: centrifuge speed of 4000-6000 rpm, centrifugation time of 10-20 min; vacuum drying temperature of 50-60 ° C for 22-26 h.

7. The method according to claim 1, in, The initial particle size of the nano calcium carbonate is 20-100 nanometers; the thickness of the high-toughness resin coating layer is 5-50 nanometers.

8. A high-toughness resin-coated nano-calcium carbonate nano-plugging agent for water-based drilling fluid, It is characterized in that The nano plugging agent is prepared by the method described in any one of claims 1 to 5, and has excellent dispersibility and plugging performance.

9. A water-based drilling fluid, It is characterized in that The invention comprises the high-toughness resin-coated nano-calcium carbonate nano-plugging agent as described in claim 8.

10. The water-based drilling fluid according to claim 9, in, The water-based drilling fluid comprises the following components: 100 parts by weight of base fluid, 7-13 parts by weight of bentonite, 0.6-1.4 parts by weight of polymer viscosity enhancer, 3-9 parts by weight of fluid loss reducer, 3-7 parts by weight of conventional plugging agent, 1-5 parts by weight of lubricant, 4-8 parts by weight of inhibitor, 1.5-2.5 parts by weight of pH adjuster, 0.5-1.5 parts by weight of nano plugging agent and 80-300 parts by weight of weighting agent.

Citation Information

Patent Citations

  • Preparation method of modified nano calcium carbonate

    CN101525146A

  • Surface modified nano calcium carbonate with core-shell structure and preparation method thereof

    CN104559327A

  • Surface modification process for nano-calcium carbonate by composite modifier

    CN109504131A

  • Method for optimizing a modification process of nano calcium carbonate

    CN113461042A

  • High-temperature-resistant particle-size-variable oil-based drilling fluid composite plugging agent and preparation method thereof

    CN113583644A

Cited By

  • Sand washing temporary plugging agent and preparation method thereof

    CN120818346A