Low-cost deoxidation method for steelmaking
By optimizing the deoxidant composition of CaO, CSi, elemental silicon, elemental carbon and iron, the problems of high cost of deoxidant and poor deoxidation effect in converter steelmaking are solved, and low-cost, effective oxygen content reduction and steel quality improvement are achieved. .
Patent Information
- Application Number
- CN202411004976.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The high cost of deoxidant in existing converter steelmaking and the inclusions (such as Al2O3) generated by the steel material are affected, and the deoxidation effect of commonly used deoxidants is not thorough, resulting in the difficulty of effectively reducing the oxygen content of molten steel.
Using a deoxidant composed of CaO, CSi, elemental silicon, elemental carbon and iron, by optimizing its mass percentage and particle size, stable dicalcium silicate is generated to improve the deoxidation effect, and by controlling the iron content, the specific gravity of the deoxidant is increased to enhance the Deoxygenation capacity reduces CO gas production and reduces deoxygenation cost.
The low-cost and effective reduction of the oxygen content of molten steel is achieved, reducing the generation of Al2O3 inclusions, and the stable control of the oxygen content of molten steel is below 20ppm, reducing the cost of deoxidant and improving the quality of steel.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of converter steelmaking, and in particular relates to a low-cost deoxidation method for steelmaking. Background Art
[0002] Converter steelmaking uses oxygen blowing to remove impurities from molten steel, and the residual oxygen content in the molten steel is high. Residual oxygen in the molten steel will cause defects such as subcutaneous bubbles and looseness in the ingot, and aggravate the harm of sulfur. The generated oxide inclusions remain in the steel, which will reduce the mechanical properties of the steel such as plasticity and impact toughness. Therefore, the oxygen content of the molten steel must be removed to a lower value during the steelmaking process. Commonly used deoxidizers are aluminum, silicon and carbon deoxidizers, and the deoxidation products are mainly Al 2 O 3 、SiO 2 and CO, 1kg aluminum can remove 0.89kg oxygen, 1kg silicon can remove 1.14kg oxygen, 1kg carbon can remove 1.33kg oxygen. Under the same deoxidizing dosage, carbon deoxidizes the most and aluminum deoxidizes the least. Aluminum-based deoxidizers mainly use metal aluminum for deoxidation. The high price of aluminum blocks leads to high deoxidation costs. At the same time, the Al 2 O 3 If the inclusions cannot be removed in time, it will lead to the blockage of the water inlet during the continuous casting process and the excessive Class B inclusions in the steel. Silicon-based deoxidizers mainly use silicon carbide and ferrosilicon for deoxidation. The price is relatively cheap, but silicon carbide is relatively light and is mainly used for slag surface deoxidation. Ferrosilicon has a higher specific gravity than silicon carbide and can deoxidize molten steel. The reaction product is SiO 2 The ability of silicon to combine with oxygen is lower than that of aluminum, so there is a problem of high residual oxygen content in molten steel due to incomplete deoxidation. Carbon-based deoxidizers include calcium carbide (CaC 2 ) and carbon powder, which are relatively cheap but light in weight and are mainly used for slag surface deoxidation, and their deoxidation capacity is generally weak.
[0003] CN108588333 A A low-cost deoxidation process for converter steelmaking. In the process of converter steel tapping, carbon powder and composite deoxidizer are added for staged deoxidation. At the beginning of steel tapping, carbon powder is thrown on the top and sprayed on the bottom for the first step of deoxidation. After that, a composite deoxidizer composed of silicon, calcium and barium is added for further deoxidation, so as to achieve the purpose of reducing the deoxidation cost. The patented deoxidation process is relatively cumbersome, and the first step is to use carbon powder for deoxidation. The reaction product is all CO gas. There is a risk of molten steel splashing (overturning) during the CO gas overflow process. At the same time, the composite deoxidizer used in the deoxidation process is composed of silicon, calcium and barium, and calcium and barium are precious alloys, which limits its cost reduction. Summary of the invention
[0004] The purpose of the present invention is to provide a low-cost deoxidation method for steelmaking, which can effectively remove the oxygen content in molten steel while reducing the deoxidation cost and reduce Al 2 O 3The generation of inclusions. The specific method steps and control parameters are as follows:
[0005] A low-cost deoxidation method for steelmaking, the converter adopts conventional smelting process, and the deoxidizer is first added according to the oxygen content of the molten steel at the converter end point during the steel tapping process, and then other alloys and slag are added.
[0006] Furthermore, the deoxidizer is composed of the following components in mass percentage: CaO: 32-50%, CSi: 20-25%, elemental silicon: 20-25%, elemental carbon: 5-10%, iron: 5-10%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3 ;
[0007] Among them, silicon carbide, elemental silicon, and elemental carbon are mainly used for deoxidation and are cheap, but the content of silicon carbide and elemental carbon should not be too high, especially the content of elemental carbon should not be too high, otherwise it will easily lead to violent carbon-oxygen reaction and the risk of splashing; the calcium oxide in the ingredients is mainly used to react with the deoxidation product SiO 2 The reaction generates stable dicalcium silicate compounds to improve the deoxidation effect. If the calcium oxide content is too high, the content of other components will decrease and the deoxidation effect will become worse. If the calcium oxide content is too low, the generated SiO 2 It cannot fully combine with CaO, and the deoxidation ability is weakened; the iron in the composition is mainly used to increase the specific gravity of the deoxidizer. Low iron content leads to insufficient bulk density of the silicon-carbon alloy, which is easy to float on the slag surface and cannot effectively remove oxygen from the molten steel. High iron content will lead to less other components and poor deoxidation effect.
[0008] Furthermore, the oxygen content of the converter end point molten steel is ≤300ppm, and 0.5-1.0kg / t of deoxidizer is added; the oxygen content of the converter end point molten steel is 300-600ppm, and 1.0-1.5kg / t of deoxidizer is added; the oxygen content of the converter end point molten steel is >600ppm, and 1.5-2.0kg / t of deoxidizer is added.
[0009] Furthermore, the deoxidizer is added after 1 / 3 to 1 / 2 of the steel is tapped.
[0010] Furthermore, the alloy includes low carbon ferromanganese; and the slag includes lime.
[0011] The advantages of the present invention are mainly reflected in the following aspects:
[0012] 1. The present invention optimizes the components and ratios of the deoxidizer to obtain a low-cost deoxidizer, which is composed of the following components by mass percentage: CaO: 32-50%, CSi: 20-25%, elemental silicon: 20-25%, elemental carbon: 5-10%, iron: 5-10%; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3 The deoxidizer is composed of carbon and silicon deoxidizers with the largest deoxidation capacity, and the lowest comprehensive deoxidation cost can reach 1.5 yuan / ton of steel. The deoxidizer contains calcium oxide, which can react with the deoxidation product silicon dioxide to generate more stable dicalcium silicate, thereby improving the deoxidation effect. The deoxidizer contains metallic iron, and the specific gravity of the deoxidizer is controlled at 4.5-5.5g / cm 3 , can fully contact with molten steel to improve the deoxidation effect. The deoxidizer controls the total amount of carbon and can avoid the generation of a large amount of CO gas during the deoxidation process, which may lead to bag overturning accidents.
[0013] 2. The deoxidizer is composed of carbon and silicon deoxidizing substances, and the deoxidized product does not contain Al 2 O 3 , which can reduce the risk of water blockage during the casting process, and can reduce the generation of Class B inclusions in steel and improve the quality of steel.
[0014] 3. The present invention classifies the oxygen content at the converter end point, and further refines the management of the amount of deoxidizer used for molten steel with different oxygen contents, thereby reducing waste caused by excessive deoxidizer use or poor deoxidation effect caused by insufficient deoxidizer use.
[0015] 4. The method of the present invention can stably control the oxygen content of molten steel at the refining station to below 20ppm, the alloy yield is above 95%, and the cost of deoxidizer is greatly reduced, which is worthy of promotion and application.
[0016] 5. The deoxidation method of the present invention is applicable to all types of steel except ultra-low carbon steel (C < 0.04%). DETAILED DESCRIPTION
[0017] The present invention is further described in detail below in conjunction with embodiments and comparative examples, taking the process for preparing cold heading steel as an example.
[0018] Example 1
[0019] The 120-ton converter adopts conventional smelting process, the carbon content at the smelting end point is 0.08%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.10%, the oxygen content of molten steel is 275ppm, and 100kg of deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CaO: 38.6%, CSi: 22.3%, elemental silicon: 23.2%, elemental carbon: 6.1%, iron: 7.1%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm3 , the price is 1.8 yuan / kg. 30s after the deoxidizer is added, add 500kg lime and 500kg low carbon ferromanganese, the composition of low carbon ferromanganese is C: 0.2%, Mn: 81%, and the rest is iron and unavoidable impurities.
[0020] Molten steel volume: 120 tons, oxygen content of molten steel at refined station is 16ppm, silicon content of molten steel is 0.001%, manganese content of molten steel is 0.43%, carbon content of molten steel is 0.085%, deoxidation cost is 1.5 yuan / ton steel, and low carbon ferromanganese manganese recovery rate is 97.8%. The calculation formula of low carbon ferromanganese recovery rate is: molten steel volume*1000*(manganese content at refined station-manganese content at converter end point) / (low carbon ferromanganese dosage*low carbon ferromanganese manganese content)*100%.
[0021] Example 2
[0022] The converter adopts conventional smelting process, the carbon content at the smelting end point is 0.065%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.09%, the oxygen content of molten steel is 486ppm, and 150kg of deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CaO: 42.6%, CSi: 20.6%, elemental silicon 23.1%, elemental carbon: 5.7%, iron: 7.1%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3 , the price is 1.8 yuan / kg. 30s after the deoxidizer is added, add 500kg lime and 500kg low carbon ferromanganese, the composition of low carbon ferromanganese is C: 0.22%, Mn: 81.2%, and the rest is iron and unavoidable impurities.
[0023] The oxygen content of the refined steel at the station is 17ppm, the silicon content of the steel is 0.01%, the manganese content of the steel is 0.42%, the carbon content of the steel is 0.068%, the deoxidation cost is 2.25 yuan / ton of steel, and the manganese recovery rate of low-carbon ferromanganese is 97.5%. The calculation formula for the recovery rate of low-carbon ferromanganese is: molten steel volume*1000*(manganese content at the refined station-manganese content at the converter end) / (low-carbon ferromanganese dosage*manganese content of low-carbon ferromanganese)*100%.
[0024] Example 3
[0025] The converter adopts conventional smelting process, the carbon content at the smelting end point is 0.042%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.08%, the oxygen content of molten steel is 810ppm, and 210kg deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CaO: 45.1%, CSi: 20.2%, elemental silicon 21.9%, elemental carbon: 5.2%, iron: 6.9%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3, the price is 1.8 yuan / kg. 30s after the deoxidizer is added, add 500kg lime and 500kg low carbon ferromanganese, the composition of low carbon ferromanganese is C: 0.21%, Mn: 80.6%, and the rest is iron and unavoidable impurities.
[0026] The oxygen content of the refined steel at the station is 15ppm, the silicon content of the steel is 0.008%, the manganese content of the steel is 0.41%, the carbon content of the steel is 0.043%, the deoxidation cost is 3.15 yuan / ton of steel, and the manganese recovery rate of low-carbon ferromanganese is 98.3%. The calculation formula for the recovery rate of low-carbon ferromanganese is: molten steel volume*1000*(manganese content at the refined station-manganese content at the converter end) / (low-carbon ferromanganese dosage*manganese content of low-carbon ferromanganese)*100%.
[0027] Comparative Example 1 (Compared with Example 2, silicon carbide deoxidation was used, the oxygen content at the refining station was high, the deoxidation cost was high and the alloy yield was low)
[0028] The converter adopts conventional smelting process, the carbon content at the end of smelting is 0.064%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.091%, the oxygen content of molten steel is 489ppm, and 150kg of silicon carbide is added after 40 tons of steel is tapped. The composition of silicon carbide is CSi: 75%, SiO 2 : 20%, the rest are some inevitable impurities; the price is 4.7 yuan / kg. 30s after the deoxidizer is added, add 500kg lime and 500kg low carbon ferromanganese, the composition of low carbon ferromanganese is C: 0.21%, Mn: 81.1%, the rest are iron and inevitable impurities.
[0029] The oxygen content of the refined steel at the station is 56ppm, the silicon content of the steel is 0.03%, the manganese content of the steel is 0.38%, the carbon content of the steel is 0.069%, the deoxidation cost is 5.88 yuan / ton of steel, and the manganese recovery rate of low-carbon ferromanganese is 85.5%. The calculation formula for the recovery rate of low-carbon ferromanganese is: molten steel volume*1000*(manganese content at the refined station-manganese content at the converter end) / (low-carbon ferromanganese dosage*manganese content of low-carbon ferromanganese)*100%.
[0030] Comparative Example 2 (Compared with Example 2, aluminum blocks were used for deoxidation. When the oxygen content at the refining station was similar, the deoxidation cost was significantly higher)
[0031] The converter adopts conventional smelting process, the carbon content at the end of smelting is 0.066%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.089%, the oxygen content of molten steel is 490ppm, and 80kg aluminum block is added after 40 tons of steel is tapped. The composition of aluminum block is Al: 99.5%, and the rest are some inevitable impurities; the price is 21.2 yuan / kg. 500kg lime and 500kg low-carbon ferromanganese are added 30s after the deoxidizer is added. The composition of low-carbon ferromanganese is C: 0.21%, Mn: 81.1%, and the rest are iron and inevitable impurities.
[0032] The oxygen content of the refined steel at the station is 18ppm, the silicon content of the steel is 0.01%, the manganese content of the steel is 0.41%, the carbon content of the steel is 0.069%, the deoxidation cost is 14.1 yuan / ton of steel, and the manganese recovery rate of low-carbon ferromanganese is 95.0%. The calculation formula for the recovery rate of low-carbon ferromanganese is: molten steel volume*1000*(manganese content at the refined station-manganese content at the converter end) / (low-carbon ferromanganese dosage*manganese content of low-carbon ferromanganese)*100%.
[0033] Comparative Example 3 (Compared with Example 2, the deoxidizer does not contain CaO, the oxygen content at the refining station is high, and the alloy yield is low)
[0034] The converter adopts conventional smelting process, the carbon content at the smelting end point is 0.065%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.090%, the oxygen content of molten steel is 488ppm, and 150kg of deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CSi: 20.6%, elemental silicon 23.1%, elemental carbon: 5.7%, iron: 47.3%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3 30 seconds after the deoxidizer was added, 500kg of lime and 500kg of low-carbon ferromanganese were added. The composition of low-carbon ferromanganese was C: 0.22%, Mn: 81.3%, and the rest was iron and unavoidable impurities.
[0035] The oxygen content of the refined steel at the station is 68ppm, the silicon content of the steel is 0.01%, the manganese content of the steel is 0.35%, the carbon content of the steel is 0.068%, and the manganese recovery rate of low-carbon ferromanganese is 76.8%. The calculation formula of low-carbon ferromanganese recovery rate is: steel volume*1000*(manganese content at the refined station-manganese content at the converter end point) / (low-carbon ferromanganese dosage*manganese content of low-carbon ferromanganese)*100%.
[0036] Comparative Example 4 (Compared with Example 2, the deoxidizer does not contain iron, and the specific gravity of the deoxidizer is 2.0-3.5g / cm 3 The oxygen content at the refining station is high, and the alloy yield is low)
[0037] The converter adopts conventional smelting process, the carbon content at the smelting end point is 0.062%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.085%, the oxygen content of molten steel is 495ppm, and 150kg of deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CaO: 42.6%, CSi: 20.6%, elemental silicon 23.1%, elemental carbon: 5.7%, and some unavoidable impurities; particle size: 20-50mm; specific gravity: 2.0~3.5g / cm 3 30 seconds after the deoxidizer was added, 500kg of lime and 500kg of low-carbon ferromanganese were added. The composition of low-carbon ferromanganese was C: 0.21%, Mn: 81.0%, and the rest was iron and unavoidable impurities.
[0038] The oxygen content of the refined steel at the station is 51ppm, the silicon content of the steel is 0.012%, the manganese content of the steel is 0.38%, the carbon content of the steel is 0.065%, and the manganese recovery rate of low-carbon ferromanganese is 87.4%. The calculation formula of the low-carbon ferromanganese recovery rate is: molten steel volume*1000*(manganese content at the refined station-manganese content at the converter end point) / (low-carbon ferromanganese dosage*manganese content of low-carbon ferromanganese)*100%.
[0039] Comparative Example 5 (Compared with Example 2, the carbon content in the deoxidizer was above 10%, and a slight splashing accident occurred during the steel-making process when the deoxidizer was added)
[0040] The converter adopts conventional smelting process, the carbon content at the smelting end point is 0.064%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.091%, the oxygen content of molten steel is 496ppm, and 150kg deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CaO: 42.4%, CSi: 20.6%, elemental silicon 15.3%, elemental carbon: 13.6%, iron: 7.3%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3 30 seconds after the deoxidizer was added, 500kg of lime and 500kg of low-carbon ferromanganese were added. The composition of low-carbon ferromanganese was C: 0.22%, Mn: 81.2%, and the rest was iron and unavoidable impurities.
[0041] A minor splashing accident occurred during the steel-pouring process and the test was terminated.
[0042] Comparative Example 6 (Compared with Example 2, the amount of deoxidizer used is small, the oxygen content at the refining station is high, and the alloy yield is low)
[0043] The converter adopts conventional smelting process, the carbon content at the smelting end point is 0.064%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.088%, the oxygen content of molten steel is 492ppm, and 80kg of deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CaO: 42.5%, CSi: 20.7%, elemental silicon 23.1%, elemental carbon: 5.8%, iron: 7.2%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3 , the price is 1.8 yuan / kg. 30s after the deoxidizer is added, add 500kg lime and 500kg low carbon ferromanganese, the composition of low carbon ferromanganese is C: 0.23%, Mn: 81.2%, and the rest is iron and unavoidable impurities.
[0044] The oxygen content of the refined steel at the station is 32ppm, the silicon content of the steel is 0.009%, the manganese content of the steel is 0.36%, the carbon content of the steel is 0.063%, and the manganese recovery rate of low-carbon ferromanganese is 80.39%. The calculation formula of low-carbon ferromanganese recovery rate is: steel volume*1000*(manganese content at the refined station-manganese content at the converter end point) / (low-carbon ferromanganese dosage*manganese content of low-carbon ferromanganese)*100%.
[0045] Comparative Example 7 (Compared with Example 2, the CaO content in the deoxidizer is low, the oxygen content at the refining station is high, and the alloy yield is low)
[0046] The converter adopts conventional smelting process, the carbon content at the smelting end point is 0.067%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.092%, the oxygen content of molten steel is 455ppm, and 150kg of deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CaO: 20.6%, CSi: 20.8%, elemental silicon 23.3%, elemental carbon: 6.1%, iron: 27.2%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3 30 seconds after the deoxidizer was added, 500kg of lime and 500kg of low-carbon ferromanganese were added. The composition of low-carbon ferromanganese was C: 0.23%, Mn: 81.3%, and the rest was iron and unavoidable impurities.
[0047] The oxygen content of the refined steel at the station is 41ppm, the silicon content of the steel is 0.008%, the manganese content of the steel is 0.38%, the carbon content of the steel is 0.068%, and the manganese recovery rate of low-carbon ferromanganese is 85.02%. The calculation formula of the low-carbon ferromanganese recovery rate is: molten steel volume*1000*(manganese content at the refined station-manganese content at the converter end point) / (low-carbon ferromanganese dosage*low-carbon ferromanganese manganese content)*100%.
[0048] Comparative Example 8 (Compared with Example 2, the CaO content in the deoxidizer is higher than 50%, resulting in a decrease in the content of other components, a poor deoxidation effect, a high oxygen content at the refining station, and a low alloy yield)
[0049] The converter adopts conventional smelting process, the carbon content at the smelting end point is 0.063%, the silicon content of molten steel is 0.001%, the manganese content of molten steel is 0.086%, the oxygen content of molten steel is 512ppm, and 150kg deoxidizer is added after 40 tons of steel is tapped. The composition of the deoxidizer is CaO: 63.8%, CSi: 12.3%, elemental silicon 11.1%, elemental carbon: 4.8%, iron: 7.1%, and some inevitable impurities; particle size: 20-50mm; specific gravity: 4.5-5.5g / cm 3 30 seconds after the deoxidizer was added, 500kg of lime and 500kg of low-carbon ferromanganese were added. The composition of low-carbon ferromanganese was C: 0.22%, Mn: 81.2%, and the rest was iron and unavoidable impurities.
[0050] The oxygen content of the refined steel at the station is 56ppm, the silicon content of the steel is 0.002%, the manganese content of the steel is 0.35%, the carbon content of the steel is 0.053%, and the manganese recovery rate of low-carbon ferromanganese is 78.03%. The calculation formula of low-carbon ferromanganese recovery rate is: steel volume*1000*(manganese content at the refined station-manganese content at the converter end point) / (low-carbon ferromanganese dosage*manganese content of low-carbon ferromanganese)*100%.
[0051] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A low-cost deoxidation method for steelmaking, Features: The converter adopts conventional smelting process. During the steel tapping process, deoxidizer is first added according to the oxygen content of the molten steel at the converter end point, and then other alloys and slag are added; The deoxidizer is composed of the following components in mass percentage: CaO: 32-50%, CSi: 20-25%, elemental silicon: 20-25%, elemental carbon: 5-10%, iron: 5-10%, and some inevitable impurities; particle size: 20-50mm; Specific gravity: 4.5~5.5g / cm 3 .
2. The steelmaking low-cost deoxidation method according to claim 1, Features: The oxygen content of the converter end point molten steel is ≤300ppm, and 0.5-1.0kg / t of deoxidizer is added; the oxygen content of the converter end point molten steel is 300-600ppm, and 1.0-1.5kg / t of deoxidizer is added; the oxygen content of the converter end point molten steel is >600ppm, and 1.5-2.0kg / t of deoxidizer is added.
3. The steelmaking low-cost deoxidation method according to claim 1, Features: The deoxidizer is added after 1 / 3 to 1 / 2 of the steel is tapped.
4. The steelmaking low-cost deoxidation method according to claim 1, Features: The alloy includes low carbon ferromanganese; and the slag includes lime.
Citation Information
Cited By
Steelmaking auxiliary agent, preparation method and application thereof, and steelmaking method
CN121428205A