System and method for efficiently converting iron manganese ore phase under multi-field coupling effect

Through the multi-field coupling system combined with microwave heating and fluidized roasting technology, the problem of poor separating effect of ferromanganese ore is solved, efficient conversion of ferromanganese ore is achieved, heating efficiency and magnetic conversion rate are improved, and energy consumption is reduced. Provides efficient and environmentally friendly development and utilization solutions.

CN118910398APending Publication Date: 2024-11-08SHANDONG UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410926586.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When the prior art treats co-concomitant ferromanganese ore, the sorting effect is poor, making it difficult to achieve efficient separation and enrichment, and traditional ore dressing methods have negative impacts on the environment.

Method used

Using a multi-field coupling system, combined with microwave heating and fluidized roasting technology, the efficient conversion of ferromanganese ore can be achieved through the first-level, The second- and third-level fully fluidized conversion chambers realize selective conversion of iron ore and manganese minerals respectively.

Benefits of technology

It significantly improves heating efficiency and magnetic conversion rate, reduces energy consumption, and realizes efficient conversion of iron and manganese minerals, lays a good foundation for subsequent sorting, and provides new ideas for efficient, environmentally friendly and energy-saving development and utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910398A_ABST
    Figure CN118910398A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of mineral processing, and particularly discloses a system and method for efficiently converting iron manganese ore phases under the multi-field coupling effect. The method is used for solving the problems of small selectability difference and high-efficiency separation difficulty of associated ferromanganese ore. The system for high-efficiency conversion of the iron manganese ore phase under the multi-field coupling action adopts a multi-stage fluidized bed device under the action of a microwave field, and comprises a three-chamber combined cavity, namely a first-stage sufficient fluidization heat storage heating drying chamber, a second-stage sufficient fluidization iron phase conversion chamber and a third-stage sufficient fluidization manganese phase conversion chamber, the gradient phase efficient conversion under the multi-field coupling action of a microwave field, a stress field, a gas-solid flow field, a temperature field and the like is carried out on the ferromanganese ore material, the magnetic property difference of the iron ore and the manganese ore is increased, the subsequent separation index is improved, and efficient comprehensive development and utilization of the ferromanganese ore are achieved. Compared with existing various phase conversion devices, the heating efficiency is improved by more than 10 times, and the magnetic conversion rate and the birnessite conversion rate index are both improved by more than 3%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of mineral processing, and in particular relates to a system and method for efficient conversion of iron-manganese ore phases under multi-field coupling. Background Art

[0002] my country has rich reserves of manganese resources inland and overseas, but the manganese grade of manganese ore resources in my country and overseas is low, and the associated components are complex. More than 70% of manganese ore resources are associated ferromanganese ore resources. Ferromanganese ore is an ore that contains both iron and manganese. Generally speaking, the iron content is high, usually between 10% and 40%, and the manganese content is relatively low, usually between 10% and 20%. It has the characteristics of iron-manganese isomorphism and fine-grained embedding. Due to the complex mineral composition and small selectivity differences of this type of resource, its efficient separation has always been a world-class problem. Therefore, it is of great significance to carry out basic research and cutting-edge technology exploration around the associated ferromanganese ore to achieve efficient utilization.

[0003] In order to achieve the effective separation and enrichment of iron and manganese in ferromanganese ore, there are many traditional beneficiation methods. Among them, the mechanical and physical beneficiation of ferromanganese ore is relatively simple and low-cost. However, due to the influence of the small difference in the density and magnetic properties of iron and manganese in ferromanganese ore, the effects of single gravity separation and magnetic separation are relatively poor, and the physical combined process indicators are not high, so it is difficult to achieve efficient separation by mechanical and physical beneficiation. Chemical leaching has a high extraction rate and good selectivity, and can process low-grade ores and difficult-to-process ores, but it will produce more wastewater and waste, which will have an adverse effect on equipment and the environment. Bioleaching is relatively friendly to the environment and has its unique advantages in the treatment of ferromanganese ore, but due to its long processing time, it is difficult to achieve large-scale production and application. In summary, traditional beneficiation technologies have some limitations in the treatment of ferromanganese ore, and cannot meet the clean and efficient recycling of ferromanganese ore.

[0004] With the development of modern technology, magnetization roasting technology is one of the effective means to deal with refractory iron ore resources. Among them, fluidized magnetization roasting and microwave magnetization roasting have shown their great advantages in the separation of refractory iron ore. Fluidized magnetization roasting refers to the heating and reduction of ore particles in a fluidized state under the action of a fluid medium, so as to achieve the purpose of magnetization roasting. It has the characteristics of uniform and stable product quality, good heat transfer effect, high level of process control and automation, and few equipment operating parts. In view of the low grade and many types of complex and difficult-to-separate iron ore, Northeastern University proposed a new concept of suspended magnetization roasting of iron ore "pre-oxidation-heat storage reduction-reoxidation", developed an iron ore suspended magnetization roasting laboratory and pilot equipment, and developed a new process of "pre-enrichment-suspended magnetization roasting-separation" for complex and difficult-to-separate iron ore. Suspended magnetization roasting expansion continuous tests were carried out for Sinosteel Algerian oolitic hematite, Ansteel Dong'anshan tailings, Jiugang powder ore, tailings and lump ore, all of which achieved good separation indicators. Based on the above research results, Jiugang Group built a 1.65 million tons / year suspended magnetization roasting industrial production line in March 2018.

[0005] Microwaves refer to electromagnetic waves with a frequency of 300MHz to 300GHz and a wavelength of 1mm to 1m. They can penetrate into the mineral molecules, causing heat to occur from the inside of the molecules without the need for heat conduction, with high thermal efficiency and low energy consumption. Secondly, different minerals coexisting in the same ore will also show different temperature rise changes, exacerbating the softening of their bonding surfaces. Therefore, microwave roasting has the characteristics of rapid heating, selective heating, low energy consumption, and enhanced mineral monomer dissociation and grindability, and has become a hot topic of research in recent years. The application of microwaves in the separation of iron and manganese ores will have broad development prospects.

[0006] The invention combines the microwave heating technology of selective rapid heating with the fluidized roasting technology of efficient heat and mass transfer, applies microwave heating to the fluidized magnetization roasting technology under the coupling of multiple fields such as microwave field, stress field, gas-solid flow field and temperature field, realizes heat storage and temperature-raising drying of iron-manganese ore at low temperature according to thermodynamic calculation, selectively converts weakly magnetic iron minerals in the iron-manganese ore into strongly magnetic minerals at relatively low temperature and weakly reducing atmosphere, and selectively converts hydromanganese ore and pyrolusite in the ore into shalymanganese at relatively high temperature and strong reducing atmosphere, thereby realizing efficient conversion of iron-manganese mineral phases, laying a good foundation for subsequent efficient separation of iron-manganese ore, and providing a new idea for efficient, environmentally friendly and energy-saving development and utilization of iron-manganese ore. Summary of the invention

[0007] One object of the present invention is to provide a system for efficient conversion of iron-manganese ore phases under multi-field coupling, which effectively solves the problem of small selectivity difference and difficulty in efficient separation of co-existing iron-manganese ores.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0009] A system for efficient conversion of iron-manganese ore phases under multi-field coupling, comprising: a feeding chamber, a first microwave generating device, a second microwave generating device, a first-level fully fluidized heat storage and temperature rising drying chamber, a second-level fully fluidized iron phase conversion chamber, a third-level fully fluidized manganese phase conversion chamber, a first air supply device, a second air supply device, a third air supply device, a fourth air supply device, a fifth air supply device, a temperature measuring device, a cyclone device, a power device and a collecting bin.

[0010] The first-level fully fluidized heat storage and temperature rising drying chamber, the second-level fully fluidized iron phase transformation chamber and the third-level fully fluidized manganese phase transformation chamber are connected in parallel on the left and right to form a whole, wherein each of the first-level fully fluidized heat storage and temperature rising drying chamber, the second-level fully fluidized iron phase transformation chamber and the third-level fully fluidized manganese phase transformation chamber is provided with a partition for separating the corresponding chamber left and right, and the first-level fully fluidized heat storage and temperature rising drying chamber, the second-level fully fluidized iron phase transformation chamber and the third-level fully fluidized manganese phase transformation chamber are divided into a feed chamber on the left and a discharge chamber on the right by the corresponding partition, the top of the partition is connected to the inner top wall of the corresponding chamber, and a channel for material circulation is provided between the bottom of the partition and the inner bottom wall of the corresponding chamber.

[0011] A feed port is provided at the upper portion of the left side wall of the first-stage fully fluidized heat storage and temperature rising drying chamber, and the outlet of the feeding chamber is communicated with the feed port; a discharge port is provided at the upper portion of the right side wall of the third-stage fully fluidized manganese phase conversion chamber, and the discharge port is communicated with the collecting bin; a first microwave generating device is provided at the outer side of the left side wall of the first-stage fully fluidized heat storage and temperature rising drying chamber, and a second microwave generating device is provided at the outer side of the right side wall of the third-stage fully fluidized manganese phase conversion chamber.

[0012] The bottom of the first-level fully fluidized heat storage and temperature rising drying chamber, the second-level fully fluidized iron phase conversion chamber and the third-level fully fluidized manganese phase conversion chamber are each provided with two air inlet holes, and the two air inlet holes are respectively arranged on the left and right sides of the corresponding partition, and the air inlet holes are respectively the first air inlet hole, the second air inlet hole, the third air inlet hole, the fourth air inlet hole, the fifth air inlet hole and the sixth air inlet hole from left to right.

[0013] The first air inlet and the second air inlet are both connected to the first air supply device, the third air inlet is connected to the second air supply device, the fourth air inlet is connected to the third air supply device, the fifth air inlet is connected to the fourth air supply device, and the sixth air inlet is connected to the fifth air supply device.

[0014] The first, second and third return air ports are respectively arranged on the top wall of the chamber directly above the first, third and fifth air inlet holes. The first, second and third return air ports are all connected to the inlet of the cyclone device, the outlet of the cyclone device is connected to the inlet of the feeding chamber, and the cyclone device is connected to the power device.

[0015] A thermocouple is provided in each chamber located directly above the second air inlet hole, the fourth air inlet hole and the sixth air inlet hole, and the thermocouple is connected to a temperature measuring device.

[0016] Furthermore, the volume ratio of each feed chamber to the discharge chamber is 1:5, the height of each partition is equal, and the height ratio of each partition to the corresponding chamber is 1:1.2.

[0017] Furthermore, the microwave generating device is composed of a waveguide, a magnetron and an antenna cap. The waveguide is connected to a power source through a wire. The waveguide is arranged below the magnetron. A microwave power regulator is installed on the magnetron. The antenna cap is arranged below the magnetron and inserted into the waveguide.

[0018] Another object of the present invention is to provide a method for efficient conversion of iron-manganese ore phases under multi-field coupling, which is applied to the system described in the above embodiment, and comprises the following steps: S1, crushing, grinding and mixing the iron-manganese ore sample to obtain an iron-manganese ore powder sample, and evenly feeding it into the feed chamber of a first-level fully fluidized heat storage and heating drying chamber through the feed chamber.

[0019] S2. The first gas supply device pumps protective gas through the first gas inlet hole to make the iron-manganese ore powder sample flow to the discharge chamber of the first-level fully fluidized heat storage and temperature rising drying chamber.

[0020] S3. The first gas supply device pumps protective gas through the second gas inlet hole to make the iron-manganese ore powder sample in a fluidized state in the discharge chamber of the first-level fully fluidized heat storage and heating drying chamber.

[0021] S4. Turn on the first microwave generator, and the generated microwave enters the first-level fully fluidized heat storage and temperature rising drying chamber, and heats the iron-manganese ore powder sample therein to 400-600° C. The heated iron-manganese ore powder sample is discharged from the discharge chamber of the first-level fully fluidized heat storage and temperature rising drying chamber, and enters the feed chamber of the second-level fully fluidized iron phase conversion chamber.

[0022] S5. The second gas supply device pumps protective gas through the third gas inlet hole to make the iron-manganese ore powder sample flow from the feed chamber of the secondary fully fluidized iron phase conversion chamber to the discharge chamber of the secondary fully fluidized iron phase conversion chamber.

[0023] S6. The third gas supply device pumps reducing gas through the fourth gas inlet hole to cause the iron-manganese ore powder sample to undergo an iron mineral phase transformation reaction in the discharge chamber of the secondary fully fluidized iron phase transformation chamber, and the fluidized iron-manganese ore powder sample is sent into the feed chamber of the tertiary fully fluidized manganese phase transformation chamber.

[0024] S7. The fourth gas supply device pumps protective gas through the fifth gas inlet hole to make the iron-manganese ore powder sample flow from the feed chamber of the three-stage fully fluidized manganese phase conversion chamber to the discharge chamber of the three-stage fully fluidized manganese phase conversion chamber.

[0025] S8. Turn on the second microwave generator, and the microwave generated enters the three-stage fully fluidized manganese phase conversion chamber, and heats the iron-manganese ore powder sample therein to 600-800°C. At the same time, the fifth gas supply device pumps reducing gas into the sixth gas inlet hole, so that the iron-manganese ore powder sample undergoes a manganese mineral phase conversion reaction in the three-stage fully fluidized manganese phase conversion chamber, and the fluidized iron-manganese ore powder sample is discharged through the discharge port of the three-stage fully fluidized manganese phase conversion chamber and enters the collecting bin, so as to obtain an iron-manganese ore product that has undergone phase conversion.

[0026] Furthermore, in step S1, the ferromanganese ore sample is first crushed to a particle size of ≤2 mm, and then ground to a particle size of ≤0.074 mm accounting for 40% to 90% of the total mass of the ferromanganese ore sample to prepare an ferromanganese ore powder sample.

[0027] Furthermore, the iron grade of the ferromanganese ore sample is 10% to 60%, the manganese grade is 1% to 30%, and the protective gas is N 2 or CO 2 The reducing gas is CO, H 2 , CH 4 Or water gas.

[0028] Furthermore, the residence time of the iron-manganese ore powder sample in the first-level fully fluidized heat storage and heating drying chamber is 10 to 90 minutes, the residence time of the heated iron-manganese ore powder sample in the second-level fully fluidized iron phase transformation chamber is 10 to 90 minutes, and the residence time of the iron-manganese ore powder sample in the third-level fully fluidized manganese phase transformation chamber is 10 to 90 minutes.

[0029] Further, in step S6, when reducing gas is introduced into the discharge chamber of the secondary fully fluidized iron phase conversion chamber, the volume ratio of the amount of reducing gas introduced to the amount of protective gas introduced into the feed chamber of the secondary fully fluidized iron phase conversion chamber is 1:10 to 2:6.

[0030] In step S8, when reducing gas is introduced into the discharge chamber of the three-stage fully fluidized manganese phase conversion chamber, the volume ratio of the amount of reducing gas introduced to the amount of protective gas introduced into the feed chamber of the three-stage fully fluidized manganese phase conversion chamber is 1:10 to 2:6.

[0031] Furthermore, after the manganese mineral phase conversion reaction is completed, first, stop introducing the reducing gas into the discharge chamber of the secondary fully fluidized iron phase conversion chamber and the discharge chamber of the tertiary fully fluidized manganese phase conversion chamber, and turn off the first microwave generator and the second microwave generator; then, stop introducing the protective gas.

[0032] Compared with the prior art, the beneficial technical effects of the present invention are:

[0033] (1) Compared with various existing phase conversion devices, the heating efficiency of the present invention is improved by more than 10 times, and the magnetic conversion rate and the conversion rate of schistosity are both improved by more than 3%.

[0034] (2) The present invention not only combines the advantages of fluidized roasting and microwave heating, but also respectively sets up a first-level fully fluidized heat storage and temperature rising drying chamber, a second-level fully fluidized iron phase transformation chamber and a third-level fully fluidized manganese phase transformation chamber, so that the iron minerals in the ferromanganese ore can achieve efficient mineral phase transformation at low temperature and low reduction concentration, and the manganese minerals in the ferromanganese ore can achieve efficient mineral phase transformation at high temperature and high reduction concentration, which is conducive to the precise control of the physical phase according to the ore characteristics.

[0035] (3) The present invention adopts a dual microwave generating device and a three-chamber connected design, which is conducive to accurately controlling the temperature required for the phase transformation process and reducing energy loss. While achieving precise control of the phase, energy consumption is also reduced by more than 20%. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the system structure of Example 1.

[0037] List of reference numerals: feeding chamber-1; first microwave generating device-2; second microwave generating device-3; first-level fully fluidized heat storage and temperature rising drying chamber-4; second-level fully fluidized iron phase conversion chamber-5; third-level fully fluidized manganese phase conversion chamber-6; first air supply device-7; second air supply device-8; third air supply device-9; fourth air supply device-10; fifth air supply device-11; temperature measuring device-12; cyclone device-13; power device-14; collecting bin-15; first partition plate-16; second partition plate-17; third partition plate-18; first air inlet hole-19; second air inlet hole-20; third air inlet hole-21; fourth air inlet hole -22; fifth air inlet -23; sixth air inlet -24; first return air outlet -25; second return air outlet -26; third return air outlet -27; thermocouple -28; waveguide -29; magnetron -30; antenna cap -31; power supply -32; microwave power regulator -33; feed chamber -41 of the first-level fully fluidized heat storage and heating drying chamber; discharge chamber -42 of the first-level fully fluidized heat storage and heating drying chamber; feed chamber -51 of the second-level fully fluidized iron phase transformation chamber; discharge chamber -52 of the second-level fully fluidized iron phase transformation chamber; feed chamber -61 of the third-level fully fluidized manganese phase transformation chamber; discharge chamber -62 of the third-level fully fluidized manganese phase transformation chamber. DETAILED DESCRIPTION

[0038] Example 1: A system for efficient conversion of iron-manganese ore phases under multi-field coupling, such as Figure 1 As shown, it includes: a feeding chamber 1, a first microwave generating device 2, a second microwave generating device 3, a first-level fully fluidized heat storage and temperature rising drying chamber 4, a second-level fully fluidized iron phase conversion chamber 5, a third-level fully fluidized manganese phase conversion chamber 6, a first air supply device 7, a second air supply device 8, a third air supply device 9, a fourth air supply device 10, a fifth air supply device 11, a temperature measuring device 12, a cyclone device 13, a power device 14 and a collecting bin 15.

[0039] The first-stage fully fluidized heat storage and temperature rising drying chamber 4, the second-stage fully fluidized iron phase transformation chamber 5 and the third-stage fully fluidized manganese phase transformation chamber 6 are three-chamber connected cavities. The first-stage fully fluidized heat storage and temperature rising drying chamber 4, the second-stage fully fluidized iron phase transformation chamber 5 and the third-stage fully fluidized manganese phase transformation chamber 6 are connected in parallel as a whole, wherein the first-stage fully fluidized heat storage and temperature rising drying chamber 4 is provided with a first partition plate 16, the second-stage fully fluidized iron phase transformation chamber 5 is provided with a second partition plate 17, and the third-stage fully fluidized manganese phase transformation chamber 6 is provided with a third partition plate 18.

[0040] The first partition 16 divides the first-stage fully fluidized heat storage and temperature-raising drying chamber 4 into a feed chamber 41 located on the left and a discharge chamber 42 located on the right, the second partition 17 divides the second-stage fully fluidized iron phase conversion chamber 5 into a feed chamber 51 located on the left and a discharge chamber 52 located on the right, and the third partition 18 divides the third-stage fully fluidized manganese phase conversion chamber 6 into a feed chamber 61 located on the left and a discharge chamber 62 located on the right. In this embodiment, the volume ratio of each feed chamber to the discharge chamber is 1:5.

[0041] The tops of the first partition 16, the second partition 17 and the third partition 18 are all connected to the inner top wall of the corresponding chamber, and the bottoms of the first partition 16, the second partition 17 and the third partition 18 are all provided with channels for material circulation between the inner bottom wall of the corresponding chamber. In this embodiment, the heights of the first partition 16, the second partition 17 and the third partition 18 are all equal, and the height ratio of each partition to the corresponding chamber is 1:1.2.

[0042] A feed port is provided on the upper left side wall of the first-stage fully fluidized heat storage and heating drying chamber 4, and the outlet of the feeding chamber 1 is connected to the feed port. A discharge port is provided on the upper right side wall of the third-stage fully fluidized manganese phase conversion chamber 6, and the discharge port is connected to the collection bin 15.

[0043] A first microwave generator 2 is provided on the outer side of the left wall of the first-stage fully fluidized heat storage and temperature rising drying chamber 4, and a second microwave generator 3 is provided on the outer side of the right wall of the third-stage fully fluidized manganese phase conversion chamber 6. The first microwave generator 2 is not in contact with the first-stage fully fluidized heat storage and temperature rising drying chamber 4, and the second microwave generator 3 is not in contact with the third-stage fully fluidized manganese phase conversion chamber 6. Both the first microwave generator 2 and the second microwave generator 3 are heated by microwave radiation.

[0044] The first-stage fully fluidized heat storage and temperature rising drying chamber 4, the second-stage fully fluidized iron phase transformation chamber 5 and the third-stage fully fluidized manganese phase transformation chamber 6 are each provided with two air inlet holes at the bottom, and the two air inlet holes are respectively arranged on the left and right sides of the corresponding partition, and the air inlet holes are respectively the first air inlet hole 19, the second air inlet hole 20, the third air inlet hole 21, the fourth air inlet hole 22, the fifth air inlet hole 23 and the sixth air inlet hole 24 from left to right. That is, the first air inlet 19 is located in the feed chamber 41 of the first-level fully fluidized heat storage and heating drying chamber 4, the second air inlet 20 is located in the discharge chamber 42 of the first-level fully fluidized heat storage and heating drying chamber 4, the third air inlet 21 is located in the feed chamber 51 of the second-level fully fluidized iron phase transformation chamber 5, the fourth air inlet 22 is located in the discharge chamber 52 of the second-level fully fluidized iron phase transformation chamber 5, the fifth air inlet 23 is located in the feed chamber 61 of the tertiary fully fluidized manganese phase transformation chamber 6, and the sixth air inlet 24 is located in the discharge chamber 62 of the tertiary fully fluidized manganese phase transformation chamber 6.

[0045] The first air inlet hole 19 and the second air inlet hole 20 are both connected to the first air supply device 7, the third air inlet hole 21 is connected to the second air supply device 8, the fourth air inlet hole 22 is connected to the third air supply device 9, the fifth air inlet hole 23 is connected to the fourth air supply device 10, and the sixth air inlet hole 24 is connected to the fifth air supply device 11.

[0046] The first return air port 25, the second return air port 26 and the third return air port 27 are respectively arranged on the top wall of the chamber located directly above the first air inlet 19, the third air inlet 21 and the fifth air inlet 23, that is, the first return air port 25, the second return air port 26 and the third return air port 27 are respectively arranged on the top wall of the feed chamber 41 of the first-level fully fluidized heat storage and temperature rising drying chamber 4, the feed chamber 51 of the second-level fully fluidized iron phase conversion chamber 5, and the feed chamber 61 of the third-level fully fluidized manganese phase conversion chamber 6. The first return air port 25, the second return air port 26 and the third return air port 27 are all connected to the inlet of the cyclone device 13, the outlet of the cyclone device 13 is connected to the inlet of the feed chamber 1, and the cyclone device 13 is connected to the power device 14.

[0047] A thermocouple 28 is provided in the chamber directly above the second air inlet 20, the fourth air inlet 22 and the sixth air inlet 24, and each thermocouple 28 is connected to the temperature measuring device 12, that is, a first temperature measuring point, a second temperature measuring point and a third temperature measuring point are respectively provided in the discharge chamber 42 of the first-level fully fluidized heat storage and heating drying chamber 4, the discharge chamber 52 of the second-level fully fluidized iron phase conversion chamber 5 and the discharge chamber 62 of the tertiary fully fluidized manganese phase conversion chamber 6.

[0048] In this embodiment, the microwave generating device is composed of a waveguide 29, a magnetron 30 and an antenna cap 31. The waveguide 29 is connected to a power supply 32 through a wire. The waveguide 29 is arranged below the magnetron 30. The magnetron 30 is equipped with a microwave power regulator 33. The antenna cap 31 is arranged below the magnetron 30 and inserted into the waveguide 29.

[0049] Example 2: A method for efficient conversion of iron-manganese ore phase under multi-field coupling, applied to the system described in Example 1. The iron grade of the iron-manganese ore sample used in this example is 36.5%, the manganese grade is 13.66%; the main impurity components are SiO 2 and Al 2 O 3 , the contents are 8.32% and 2.55% respectively; the relative content of hematite is 55.65%; the manganese minerals are mainly pyrolusite (MnO 2 ) and brown manganese ore (Mn 2 O 3 ), with relative contents of 15.75% and 3.64% respectively; the gangue minerals are mainly quartz.

[0050] The method comprises the following steps: S1, crushing the iron manganese ore sample to a particle size of ≤2 mm, grinding the ore to a particle size of ≤0.074 mm, which accounts for 60% of the total mass, and then mixing the mixture evenly to obtain an iron manganese ore powder sample, which is evenly fed into the feed chamber 41 of the first-level fully fluidized heat storage and temperature rising drying chamber 4 through the feed chamber 1.

[0051] S2, the first gas supply device 7 pumps in protective gas N through the first gas inlet hole 19 2 , so that the iron-manganese ore powder sample flows to the discharge chamber 42 of the first-level fully fluidized heat storage and temperature rising drying chamber 4.

[0052] S3, the first gas supply device 7 pumps in protective gas N through the second gas inlet hole 20 2 , so that the iron-manganese ore powder sample is in a fluidized state in the discharge chamber 42 of the first-level fully fluidized heat storage and heating drying chamber 4.

[0053] S4, turn on the first microwave generating device 2, the microwave generated enters the primary fully fluidized heat storage and temperature rising drying chamber 4, and heats the iron-manganese ore powder sample therein to 550° C. The heated iron-manganese ore powder sample is discharged from the discharge chamber 42 of the primary fully fluidized heat storage and temperature rising drying chamber 4, and enters the feed chamber 51 of the secondary fully fluidized iron phase conversion chamber 5.

[0054] S5, the second gas supply device 8 pumps in the protective gas N through the third gas inlet hole 21 2 , so that the iron-manganese ore powder sample flows from the feed chamber 51 of the secondary fully fluidized iron phase conversion chamber 5 to the discharge chamber 52 of the secondary fully fluidized iron phase conversion chamber 5 .

[0055] S6, the third gas supply device 9 pumps the reducing gas H into the air through the fourth air inlet 22. 2 , so that the iron-manganese ore powder sample undergoes an iron mineral phase conversion reaction in the discharge chamber 52 of the secondary fully fluidized iron phase conversion chamber 5, and the fluidized iron-manganese ore powder sample is sent into the feed chamber 61 of the tertiary fully fluidized manganese phase conversion chamber 6.

[0056] S7, the fourth gas supply device 10 pumps in the protective gas N through the fifth gas inlet hole 23 2 , so that the iron-manganese ore powder sample flows from the feed chamber 61 of the three-stage fully fluidized manganese phase conversion chamber 6 to the discharge chamber 62 of the three-stage fully fluidized manganese phase conversion chamber 6.

[0057] S8, turn on the second microwave generator 3, the microwave generated enters the third-stage fully fluidized manganese phase conversion chamber 6, and heats the iron-manganese ore powder sample in it to 700° C. At the same time, the fifth gas supply device 11 pumps in reducing gas H through the sixth gas inlet 24. 2, so that the iron-manganese ore powder sample undergoes a manganese mineral phase transformation reaction in the three-stage fully fluidized manganese phase transformation chamber 6, and the fluidized iron-manganese ore powder sample is discharged through the discharge port of the three-stage fully fluidized manganese phase transformation chamber 6 and enters the collecting bin 15, so as to obtain an iron-manganese ore product with efficient phase transformation.

[0058] The residence time of the iron-manganese ore powder sample in the primary fully fluidized heat storage and heating drying chamber 4 is 45 minutes. The residence time of the heated iron-manganese ore powder sample in the secondary fully fluidized iron phase conversion chamber 5 is 45 minutes. The residence time of the iron-manganese ore powder sample in the tertiary fully fluidized manganese phase conversion chamber 6 is 45 minutes.

[0059] In step S6, when reducing gas is introduced into the discharge chamber 52 of the secondary fully fluidized iron phase conversion chamber 5, the volume ratio of the amount of reducing gas introduced to the amount of protective gas introduced into the feed chamber 51 of the secondary fully fluidized iron phase conversion chamber 5 is 2:6.

[0060] In step S8, when reducing gas is introduced into the discharge chamber 62 of the three-stage fully fluidized manganese phase conversion chamber 6, the volume ratio of the amount of reducing gas introduced to the amount of protective gas introduced into the feed chamber 61 of the three-stage fully fluidized manganese phase conversion chamber 6 is 2:6.

[0061] When the manganese mineral phase conversion reaction is completed, first, stop introducing the reducing gas into the discharge chamber 52 of the secondary fully fluidized iron phase conversion chamber 5 and the discharge chamber 62 of the tertiary fully fluidized manganese phase conversion chamber 6, and turn off the first microwave generating device 2 and the second microwave generating device 3; then, stop introducing the protective gas.

[0062] The magnetic conversion rate of iron ore in the ferromanganese ore product obtained in this embodiment is 95%, and the conversion rate of harzburgite is ≥94%.

[0063] Example 3: The difference between this example and Example 2 is that (1) in step S1, the iron manganese ore sample is crushed to a particle size of ≤2 mm and ground to a particle size of ≤0.074 mm, accounting for 50% of the total mass. (2) in step S4, the first microwave generator 2 is turned on, and the microwaves generated enter the first-level fully fluidized heat storage and heating drying chamber 4, and the iron manganese ore powder sample in the first-level fully fluidized heat storage and heating drying chamber 4 is heated to 600°C. (3) in step S8, the second microwave generator 3 is turned on, and the microwaves generated enter the third-level fully fluidized manganese phase conversion chamber 5, and the iron manganese ore powder sample in the third-level fully fluidized manganese phase conversion chamber 5 is heated to 800°C. (4) The residence time of the iron manganese ore powder sample in the first-level fully fluidized heat storage and heating drying chamber 4 is 90 minutes. The residence time of the heated iron manganese ore powder sample in the second-level fully fluidized iron phase conversion chamber 5 is 90 minutes. The residence time of the iron manganese ore powder sample in the third-level fully fluidized manganese phase conversion chamber 6 is 90 minutes. (5) In step S6, when the reducing gas is introduced into the discharge chamber 52 of the secondary fully fluidized iron phase conversion chamber 5, the volume ratio of the amount of the reducing gas introduced to the amount of the protective gas introduced into the feed chamber 51 of the secondary fully fluidized iron phase conversion chamber 5 is 1:10. In step S8, when the reducing gas is introduced into the discharge chamber 62 of the tertiary fully fluidized manganese phase conversion chamber 6, the volume ratio of the amount of the reducing gas introduced to the amount of the protective gas introduced into the feed chamber 61 of the tertiary fully fluidized manganese phase conversion chamber 6 is 1:10.

[0064] The magnetic conversion rate of iron ore in the ferromanganese ore product obtained in this embodiment is 96%, and the conversion rate of harzburgite is ≥96%.

[0065] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A system for efficient conversion of iron and manganese ore phases under multi-field coupling. It is characterized in that include: A feeding chamber, a first microwave generating device, a second microwave generating device, a first-level fully fluidized heat storage and temperature rising drying chamber, a second-level fully fluidized iron phase conversion chamber, a third-level fully fluidized manganese phase conversion chamber, a first air supply device, a second air supply device, a third air supply device, a fourth air supply device, a fifth air supply device, a temperature measuring device, a cyclone device, a power device and a collecting bin; The first-level fully fluidized heat storage and temperature rising drying chamber, the second-level fully fluidized iron phase transformation chamber and the third-level fully fluidized manganese phase transformation chamber are connected in parallel on the left and right to form a whole, wherein each of the first-level fully fluidized heat storage and temperature rising drying chamber, the second-level fully fluidized iron phase transformation chamber and the third-level fully fluidized manganese phase transformation chamber is provided with a partition for separating the corresponding chamber on the left and right, and the first-level fully fluidized heat storage and temperature rising drying chamber, the second-level fully fluidized iron phase transformation chamber and the third-level fully fluidized manganese phase transformation chamber are divided into a feed chamber on the left and a discharge chamber on the right by the corresponding partition, the top of the partition is connected to the inner top wall of the corresponding chamber, and a channel for material circulation is provided between the bottom of the partition and the inner bottom wall of the corresponding chamber; A feed port is provided at the upper portion of the left side wall of the first-stage fully fluidized heat storage and temperature rising drying chamber, and the outlet of the feed chamber is connected to the feed port; a discharge port is provided at the upper portion of the right side wall of the third-stage fully fluidized manganese phase conversion chamber, and the discharge port is connected to the collecting bin; a first microwave generator is provided at the outer side of the left side wall of the first-stage fully fluidized heat storage and temperature rising drying chamber, and a second microwave generator is provided at the outer side of the right side wall of the third-stage fully fluidized manganese phase conversion chamber; The bottom of the first-stage fully fluidized heat storage and temperature-raising drying chamber, the second-stage fully fluidized iron phase conversion chamber, and the third-stage fully fluidized manganese phase conversion chamber are each provided with two air inlet holes, and the two air inlet holes are respectively provided on the left and right sides of the corresponding partition, and the air inlet holes are respectively the first air inlet hole, the second air inlet hole, the third air inlet hole, the fourth air inlet hole, the fifth air inlet hole, and the sixth air inlet hole from left to right; The first air inlet and the second air inlet are both connected to the first air supply device, the third air inlet is connected to the second air supply device, the fourth air inlet is connected to the third air supply device, the fifth air inlet is connected to the fourth air supply device, and the sixth air inlet is connected to the fifth air supply device; A first return air port, a second return air port and a third return air port are respectively arranged on the top wall of the chamber directly above the first air inlet, the third air inlet and the fifth air inlet, the first return air port, the second return air port and the third return air port are all connected to the inlet of the cyclone device, the outlet of the cyclone device is connected to the inlet of the feeding chamber, and the cyclone device is connected to the power device; A thermocouple is provided in each chamber located directly above the second air inlet hole, the fourth air inlet hole and the sixth air inlet hole, and the thermocouple is connected to a temperature measuring device.

2. The system for efficient conversion of iron-manganese ore phases under multi-field coupling according to claim 1, It is characterized in that The volume ratio of each feed chamber to the discharge chamber is 1:5, the height of each partition is equal, and the height ratio of each partition to the corresponding chamber is 1:1.

2.

3. The system for efficient conversion of iron-manganese ore phase under multi-field coupling according to claim 2, It is characterized in that The microwave generating device is composed of a waveguide, a magnetron and an antenna cap. The waveguide is connected to a power source through a wire. The waveguide is arranged below the magnetron. A microwave power regulator is mounted on the magnetron. The antenna cap is arranged below the magnetron and inserted into the waveguide.

4. A method for efficient conversion of iron-manganese ore phases under multi-field coupling, It is characterized in that The system applied to any one of claims 1 to 3 comprises the following steps: S1. Crushing, grinding and mixing the iron-manganese ore sample to obtain the iron-manganese ore powder sample, and evenly feeding it into the feeding chamber of the first-level fully fluidized heat storage and heating drying chamber through the feeding chamber; S2, the first gas supply device pumps protective gas through the first gas inlet hole to make the iron-manganese ore powder sample flow to the discharge chamber of the first-level fully fluidized heat storage and temperature rising drying chamber; S3, the first gas supply device pumps protective gas through the second gas inlet hole, so that the iron-manganese ore powder sample is in a fluidized state in the discharge chamber of the first-level fully fluidized heat storage and heating drying chamber; S4, turning on the first microwave generator, the microwaves generated enter the primary fully fluidized heat storage and temperature rising drying chamber, and heat the iron-manganese ore powder sample therein to 400-600° C. The heated iron-manganese ore powder sample is discharged from the discharge chamber of the primary fully fluidized heat storage and temperature rising drying chamber, and enters the feed chamber of the secondary fully fluidized iron phase conversion chamber; S5, the second gas supply device pumps protective gas through the third gas inlet hole to make the iron-manganese ore powder sample flow from the feed chamber of the secondary fully fluidized iron phase conversion chamber to the discharge chamber of the secondary fully fluidized iron phase conversion chamber; S6, the third gas supply device pumps reducing gas through the fourth gas inlet hole to make the iron-manganese ore powder sample undergo an iron mineral phase conversion reaction in the discharge chamber of the secondary fully fluidized iron phase conversion chamber, and the fluidized iron-manganese ore powder sample is sent to the feed chamber of the tertiary fully fluidized manganese phase conversion chamber; S7, the fourth gas supply device pumps protective gas through the fifth gas inlet hole to make the iron-manganese ore powder sample flow from the feed chamber of the three-stage fully fluidized manganese phase conversion chamber to the discharge chamber of the three-stage fully fluidized manganese phase conversion chamber; S8. Turn on the second microwave generator, and the microwave generated enters the three-stage fully fluidized manganese phase conversion chamber, and heats the iron-manganese ore powder sample therein to 600-800°C. At the same time, the fifth gas supply device pumps reducing gas into the sixth gas inlet hole, so that the iron-manganese ore powder sample undergoes a manganese mineral phase conversion reaction in the three-stage fully fluidized manganese phase conversion chamber, and the fluidized iron-manganese ore powder sample is discharged through the discharge port of the three-stage fully fluidized manganese phase conversion chamber and enters the collecting bin, so as to obtain an iron-manganese ore product that has undergone phase conversion.

5. The method for efficient conversion of iron-manganese ore phase under multi-field coupling according to claim 4, It is characterized in that In step S1, the ferromanganese ore sample is first crushed to a particle size of ≤2 mm, and then ground to a particle size of ≤0.074 mm accounting for 40% to 90% of the total mass of the ferromanganese ore sample to prepare an ferromanganese ore powder sample.

6. The method for efficient conversion of iron-manganese ore phase under multi-field coupling according to claim 5, It is characterized in that The iron grade of the iron-manganese ore sample is 10% to 60%, and the manganese grade is 1% to 30%. The protective gas is N 2 or CO 2 The reducing gas is CO, H 2 , CH 4 Or water gas.

7. The method for efficient conversion of iron-manganese ore phase under multi-field coupling according to claim 6, It is characterized in that The residence time of the iron-manganese ore powder sample in the first-level fully fluidized heat storage and heating drying chamber is 10 to 90 minutes, the residence time of the heated iron-manganese ore powder sample in the second-level fully fluidized iron phase conversion chamber is 10 to 90 minutes, and the residence time of the iron-manganese ore powder sample in the third-level fully fluidized manganese phase conversion chamber is 10 to 90 minutes.

8. The method for efficient conversion of iron-manganese ore phase under multi-field coupling according to claim 7, It is characterized in that In step S6, when the reducing gas is introduced into the discharge chamber of the secondary fully fluidized iron phase conversion chamber, the volume ratio of the reducing gas introduced to the protective gas introduced into the feed chamber of the secondary fully fluidized iron phase conversion chamber is 1:10 to 2:6; In step S8, when reducing gas is introduced into the discharge chamber of the three-stage fully fluidized manganese phase conversion chamber, the volume ratio of the amount of reducing gas introduced to the amount of protective gas introduced into the feed chamber of the three-stage fully fluidized manganese phase conversion chamber is 1:10 to 2:

6.

9. The method for efficient conversion of iron-manganese ore phase under multi-field coupling according to claim 8, It is characterized in that When the manganese mineral phase conversion reaction is completed, first, stop introducing the reducing gas into the discharge chamber of the secondary fully fluidized iron phase conversion chamber and the discharge chamber of the tertiary fully fluidized manganese phase conversion chamber, and turn off the first microwave generator and the second microwave generator; then, stop introducing the protective gas.

Citation Information

Patent Citations

  • Microwave continuous suspension roasting method for strengthening dissociation of complex refractory iron ores