Metal nanowire impact welding device and method based on laser thermal coupling effect
Through the metal nanowire impact welding technology with laser thermal coupling effect, the thermal coupling effect of forward pulse laser and reverse laser is used to solve the problems of metal nanowire welding efficiency and quality, and achieve efficient and low-cost welding effect. And retain the original performance of the nanowires.
Patent Information
- Application Number
- CN202111076712.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-09-14
AI Technical Summary
The prior art is difficult to effectively improve the welding efficiency and quality of metal nanowires. Traditional welding methods have problems such as insufficient heat resistance of high-temperature heating materials, defects caused by mechanical pressure, complex coating steps of external media and high costs, and laser welding methods The heating efficiency and reliability have not yet reached the ideal state.
Using metal nanowire impact welding device based on laser thermal coupling effect, the plasma shock wave and reverse laser beam are generated by forward pulsed laser beam for local heating. Combined with the constraint layer and the protective layer, the spacing between adjacent nanowires is shortened and efficient welding is achieved. , and adjust process parameters in real time through the online monitoring system.
The quality and efficiency of metal nanowire welding are improved, the phenomenon of dummy is reduced, the original comprehensive mechanical properties of nanowires are retained to the maximum extent, high-reliability welding is achieved, and welding costs are reduced.
Smart Images

Figure CN115805367B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nano material welding, and in particular to a metal nanowire impact welding device and method based on laser thermal coupling effect. Background Art
[0002] With the rapid development of science and technology, flexible electronic devices with high flexibility and high deformation rate, such as touch screens, solar cells and light-emitting diodes, have gradually entered the field of electronics compared to traditional electronics. Flexible electronics is a new type of electronic technology that prepares organic and inorganic electronic devices on soft and ductile substrates. New flexible electronic devices should have excellent optoelectronic properties, high transparency, high conductivity and good stability. Transparent conductive electrodes are the core structural components of flexible electronic devices. Reasonable selection of transparent conductive electrode preparation materials is of great engineering significance for giving full play to the functional characteristics of flexible electronic devices. Indium tin oxide, as a traditional transparent conductive material for industrial use, has been gradually eliminated due to its many disadvantages such as scarce material resources, high material brittleness and high preparation cost. Among the many candidate transparent conductive electrode preparation materials (such as carbon nanotubes, graphene, conductive polymers, metal grids and metal nanowires), metal nanowires have become the preferred material for the next generation of transparent conductive films because of their excellent conductivity, bendability and low preparation cost.
[0003] The conductive mechanism of metal nanowire transparent conductive film is that the metal nanowires are randomly arranged to form a conductive network. The virtual connection phenomenon between spatially interlaced metal nanowires is the direct and main reason why the transparent conductive film prepared by them has a large surface resistance and poor deformation. Therefore, the key process for preparing high-reliability metal nanowire transparent conductive electrodes lies in the effective welding of metal nanowire contact nodes. At present, the main technical bottleneck restricting the further application of metal nanowires in the field of flexible electronics is how to further improve the welding efficiency and welding quality of spatially interlaced metal nanowires. Traditional welding methods for metal nanowires, such as high-temperature heating, mechanical pressure, and introduction of external media, can reduce the node resistance of metal nanowires to a certain extent. However, due to the differences in the thermophysical performance parameters between metal nanowires and flexible substrate materials, there are still great difficulties in the composite preparation process and mass engineering application of flexible transparent conductive films. Specifically, the upper limit of the heat-resistant temperature of the PET substrate material of conventional flexible films is low and cannot withstand the actual high-temperature operation of 200°C of metal nanowires; in the welding process of metal nanowires achieved by mechanical pressure, under the action of extremely high compressive stress (often up to 81GPa), metal nanowires have defects such as warping, slippage and peeling, which are not suitable for large, brittle and soft substrate materials. In addition, there are high requirements for industrial coating equipment, and the integrated welding cost of metal nanowires is high; the method of preparing conductive films by introducing external media (such as PEDOT:PSS, HAuCl4, etc.) will have the disadvantages of complicated film coating steps on the one hand, low film transmittance and large fog on the other hand, and will also damage the protective layer around the nanowires. Therefore, how to propose a novel metal nanowire welding method to achieve high weldability of metal nanowires is one of the problems that need to be solved urgently at this stage.
[0004] Laser processing has many advantages such as clean and environmental protection, high power density, good controllability and high processing efficiency. It is considered to be one of the most promising methods for welding metal nanowires. At present, scholars in related fields have carried out a series of research work, such as: Chinese patent with publication number CN112828470A proposes a device and method for laser beam welding of transparent glass. This method uses a laser generator to emit two pulsed lasers. The plasma generated by the laser heat source irradiating the glass will shield the subsequent laser, thereby realizing the movement of the plasma area from the laser focus area to the laser light source, thereby realizing the fusion welding between the glass. However, the heating method of this patent is to use a continuous laser beam for nonlinear heating, and the heating object is the entire material to be welded. There is room for further improvement in welding quality, energy utilization efficiency and welding efficiency. A Chinese patent with publication number CN105149781A proposes a single-point nano-welding method based on the photothermal effect. This method uses a continuous laser to output monochromatic laser and irradiate it to metal nanowires. Due to the surface plasmon characteristics, a photothermal effect is generated, thereby realizing the fusion welding of the metal nanowires. However, due to the complexity of the spatial stacking method of the metal nanowires, there will be virtual overlaps between the metal nanowires. During actual welding operations, there will inevitably be operating areas with poor welding quality, and the welding reliability needs to be further improved.
[0005] In summary, there is still no efficient and high-quality laser welding method for metal nanowires. It is urgent to propose a new laser welding method with simple welding process, low welding cost, high controllability, high welding efficiency and excellent welding quality. Summary of the invention
[0006] The purpose of the present invention is to overcome the disadvantage of poor welding quality caused by virtual overlap between spatially interlaced metal nanowires, and to provide a metal nanowire impact welding device and method based on laser thermal coupling effect, which can improve the welding quality and welding efficiency of metal nanowires while achieving the weldability of metal nanowires.
[0007] To achieve the above object, the present invention provides the following solutions:
[0008] A metal nanowire impact welding device based on laser thermal-mechanical coupling effect includes a laser, a metal nanowire and an online monitoring system;
[0009] The laser emits a forward laser beam to perform a forward indirect impact operation on the metal nanowire;
[0010] At the same time, the laser emits a reverse laser beam to perform reverse direct heating on the metal nanowires;
[0011] The upper part of the metal nanowire is provided with a constraint layer, an absorption layer and a protection layer in order from top to bottom, and the lower part of the metal nanowire is provided with a constraint layer;
[0012] The online monitoring system is used to monitor the changes in the welding behavior of metal nanowires in real time.
[0013] Furthermore, the forward laser beam directly irradiates the absorption layer to generate a plasma shock wave, which indirectly acts on the metal nanowires through the protective layer, and under the constraint of the constraint layers on both sides of the metal nanowires, punches the metal nanowires to shorten the distance between adjacent nanowires; the reverse laser beam irradiates the metal nanowires to achieve effective heating of the node area of adjacent metal nanowires, and the node area is an area with a diameter less than 1 micron with the center of the nanowire overlap point as the center.
[0014] Furthermore, the forward laser beam is a pulsed laser, and the reverse laser beam can be either a continuous laser or a pulsed laser.
[0015] Furthermore, the positive and negative laser beams can be generated separately by means of two lasers, or can be generated by means of one laser; the method of generating the positive and negative laser beams by means of one laser is: using any three or more optical path management elements among a beam expander, a beam splitter, a reflector or a focusing mirror to divide a single laser beam into two laser beams.
[0016] Furthermore, the constraint layer above the metal nanowires is any one of transparent ceramics, BK-7 glass or quartz glass; the constraint layer below the metal nanowires is any one of transparent ceramics, BK-7 glass, quartz glass or a flexible transparent substrate; the absorption layer is any one of graphite, black paint, black tape or a light-absorbing metal film; the protective layer is any one of pure metal or its alloy materials with a yield strength lower than 500 MPa.
[0017] Furthermore, the online monitoring system includes a spectrometer and a high-speed camera; the spectrometer is used to observe the dark field scattering spectrum during the metal nanowire welding process in real time, and the high-speed camera is used to observe the morphology changes during the dynamic welding process of the metal nanowires in real time; the online monitoring system is used to provide real-time feedback on the welding conditions of the metal nanowires, and then adjust the process parameters of the laser in real time to achieve closed-loop feedback of the metal nanowire impact welding process; the process parameters of the laser are laser power density, laser frequency, laser wavelength, laser pulse width, laser scanning path, laser scanning speed and the operating distance between the laser light source and the metal nanowires.
[0018] The present invention also provides a metal nanowire impact welding method based on laser thermal coupling effect, which is characterized by comprising the following steps:
[0019] Step S1. coating metal nanowires on the surface of the constrained layer;
[0020] Step S2. Laying a protective layer material with a pre-set absorption layer on the surface above the metal nanowires;
[0021] Step S3. Laying another constraining layer on top of the absorbing layer;
[0022] Step S4. Turn on the laser to emit forward and reverse laser beams, and cooperate with the three-coordinate moving platform to complete the welding operation of the metal nanowires.
[0023] Furthermore, in step S4, the time delay method can be used to adjust the time of forward laser irradiation to the absorption layer and the time of reverse laser irradiation to the metal nanowires, thereby controlling the order and duration of laser thermal regulation; the laser beam intensity can also be regulated with the help of a laser energy attenuation device.
[0024] Furthermore, in step S4, the stepwise laser shock welding of the metal nanowires in the target area can be achieved by a single-point stepping method based on a fixed trajectory; the laser spot size and the number of spots can be adjusted by beam shaping or any method of a spatial light modulator to achieve a single batch laser shock welding of the metal nanowires in the target area.
[0025] Furthermore, the spot centers of the forward laser beam and the reverse laser beam coincide with each other, thereby achieving an obvious thermal coupling effect in the beam interaction area.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. Compared with the overall nonlinear heating method of bulk materials, the local heating of the node area of the staggered metal nanowires is carried out by using the laser plasmon effect, which has higher heating efficiency and more obvious heating effect;
[0028] 2. Using pulsed laser for impact operation can shorten the spacing between spatially staggered nanowires, reduce the phenomenon of virtual overlap, and enhance the heating effect;
[0029] 3. The original comprehensive mechanical properties of metal nanowires can be retained to the maximum extent without melting the metal nanowires as a whole, thus achieving high-reliability welding of spatially staggered nanowires;
[0030] 4. With the help of online monitoring equipment, the dynamic welding behavior of metal nanowires can be monitored in real time, and the welding process parameters can be optimized in real time, thereby realizing closed-loop feedback of the metal nanowire impact welding process. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the metal nanowire impact welding method based on the laser thermal-mechanical coupling effect of the present invention.
[0032] Figure 2Schematic diagram of the position change of metal nanowires during the impact welding process.
[0033] Figure 3 This is the SEM morphology of the metal nanowires before and after laser shock assisted welding of the present invention.
[0034] Figure 1 Middle: 1-forward laser beam; 2-reverse laser beam; 3-confinement layer; 4-absorption layer; 5-protection layer; 6-metal nanowire; 7-spectrometer; 8-high-speed camera. DETAILED DESCRIPTION
[0035] The technical solution and specific implementation methods of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the present invention.
[0036] For a better understanding of the present invention, the present invention is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and do not limit the scope of the present invention.
[0037] A metal nanowire impact welding device based on laser thermal coupling effect includes a laser, a metal nanowire 6 and an online monitoring system; while the laser emits a forward laser beam 1 to perform a forward indirect impact operation on the metal nanowire, a reverse laser beam 2 is emitted to perform a reverse direct heating operation on the metal nanowire; a constraint layer 3, an absorption layer 4 and a protective layer 5 are arranged in sequence from top to bottom on the upper part of the metal nanowire, and a constraint layer 3 is arranged on the lower part of the metal nanowire 6; the online monitoring system is used to monitor the changes in the welding behavior of the metal nanowire in real time. The forward laser beam 1 directly irradiates the absorption layer to generate a plasma shock wave, which indirectly acts on the metal nanowire through the protective layer, and punches the metal nanowire under the constraint of the constraint layers on both sides of the metal nanowire, shortening the distance between adjacent metal nanowires; the reverse laser beam 2 irradiates the metal nanowire to achieve effective heating of the node area of adjacent metal nanowires, and the node area is an area with a diameter range of less than 1 micron with the center of the nanowire overlap point as the center of the circle. The forward laser beam 1 is a pulsed laser, and the reverse laser beam 2 can be either a continuous laser or a pulsed laser. The positive and negative laser beams can be generated by two lasers respectively or by one laser; the method of generating the positive and negative laser beams by one laser is: using any three or more optical path management elements of a beam expander, a beam splitter, a reflector or a focusing mirror to divide a single laser beam into two laser beams. Preferably, the constraint layer 3 above the metal nanowire 6 is any one of transparent ceramic, BK-7 glass or quartz glass; the constraint layer 3 below the metal nanowire 6 is any one of transparent ceramic, BK-7 glass, quartz glass or a flexible transparent substrate; the absorption layer 4 is any one of graphite, black paint, black tape or a light-absorbing metal film; the protective layer 5 is any one of a pure metal or its alloy material with a yield strength lower than 500 MPa. The online monitoring system includes a spectrometer 7 and a high-speed camera 8; the spectrometer 7 is used to observe the dark field scattering spectrum of the metal nanowire 6 in real time during the welding process, and the high-speed camera 8 is used to observe the morphological changes of the metal nanowire 6 in real time during the dynamic welding process; the online monitoring system is used to feedback the welding status of the metal nanowire 6 in real time, and then adjust the process parameters of the laser in real time to realize the closed-loop feedback of the impact welding process of the metal nanowire 6; the process parameters of the laser are laser power density, laser frequency, laser wavelength, laser pulse width, laser scanning path, laser scanning speed and the operating distance between the laser light source and the metal nanowire. The time of irradiation of the forward laser 1 to the absorption layer and the time of irradiation of the reverse laser 2 to the metal nanowire 6 can be adjusted by time delay, so as to control the sequence and duration of laser thermal regulation; the laser beam intensity can also be regulated by means of a laser energy attenuation device. The metal nanowire 6 in the target area can be gradually laser-impacted in a fixed trajectory by a single-point stepping method; the laser spot size and the number of spots can be adjusted by beam shaping or by using a spatial light modulator to realize single batch laser-impact welding of metal nanowires in the target area.The spot centers of the forward laser beam and the reverse laser beam coincide, thereby achieving an obvious thermal coupling effect in the beam interaction area.
[0038] The specific embodiments are as follows:
[0039] Example 1: Laser welding of spatially interlaced copper metal nanowires
[0040] like Figure 1 As shown, the metal nanowire impact welding method based on the laser thermal coupling effect in this embodiment is shown. The specific implementation steps are:
[0041] S1: Using acetone solvent and ultrasonic cleaning machine, the constrained layer material quartz glass (thickness of 1 mm) is cleaned;
[0042] S2: Coating copper metal nanowires on the cleaned quartz glass surface;
[0043] S3: Laying an aluminum foil (5 μm thick) with a pre-graphite layer on the surface above the copper metal nanowires;
[0044] S4: another quartz glass (1 mm thick) is laid on the surface of the pre-placed graphite layer, and a locking device is used to further shorten the distance between the constraint layer, the absorption layer and the protective layer;
[0045] S5: Select nanosecond pulse laser (laser wavelength is 1064nm, pulse width is 7ns, pulse frequency is 1Hz, current is 10A, voltage is 670V, laser single pulse energy is). Turn on the nanosecond pulse laser, emit a pulsed laser beam, and use the interference cutoff filter to divide the pulsed laser into pulsed laser beams with wavelengths of 1064nm and 532nm, respectively. The laser with a wavelength of 1064nm is reflected by a reflector, and then focused by a focusing mirror, through quartz glass, and directly acts on the surface of the graphite layer. The other laser with a wavelength of 532nm is reflected by a reflector, and then focused by a focusing mirror on the surface of the metal nanowire. With the three-coordinate mobile platform (moving speed is 0.1mm / s), an "S" type scanning path is used to complete the welding operation of the spatially staggered copper metal nanowires in the target area.
[0046] like Figure 2 The schematic diagram of the change of the position of the metal nanowires during the impact welding process is shown. The welding mechanism of the copper metal nanowires in this embodiment is: using the reverse laser plasmon effect to perform local heating of the staggered metal nanowire node area, using the forward pulse laser to perform the impact operation, shortening the distance between adjacent nanowires, reducing the virtual overlap phenomenon, and strengthening the heating effect. In the case that the metal nanowires are not melted as a whole, the original comprehensive mechanical properties of the metal nanowires are retained to the maximum extent, and the high reliability welding operation of the spatially staggered nanowires is achieved.
[0047] like Figure 3 The figure shows the SEM morphology of copper metal nanowires before and after laser shock assisted welding in this embodiment. Observing sub-figure (a), it is found that when the forward pulse laser is not used for shock operation, that is, when only the reverse heating laser is used for irradiation operation, the welding quality of the metal nanowire is poor, and only the melting morphology appears at the end of the nanowire. Comparing sub-figure (a) and observing sub-figure (b), it is found that when the forward pulse laser is combined, that is, the forward and reverse laser beams are used for processing at the same time, the large-area welding of spatially staggered nanowires is achieved.
[0048] Example 2: Laser welding of spatially staggered copper metal nanowires on a polyethylene terephthalate (PET) substrate
[0049] like Figure 1 As shown, the metal nanowire impact welding method based on the laser thermal coupling effect in this embodiment is shown. The specific implementation steps are:
[0050] S1: Use ethanol and distilled water and use an ultrasonic cleaner to clean the PET substrate material for 10 minutes.
[0051] S2: Use a rod coater to evenly coat the copper metal nanowires on the surface of the PET substrate.
[0052] S3: Laying an aluminum foil (5 μm thick) with a pre-graphite layer on the surface above the copper metal nanowires;
[0053] S4: Using a BK-7 cylindrical roller, the PET substrate, copper metal nanowires, and aluminum foil with a pre-graphite layer were rolled in real time;
[0054] S5: Select nanosecond pulse laser (laser wavelength is 1064nm, pulse width is 7ns, pulse frequency is 1Hz, current is 10A, voltage is 670V, laser single pulse energy is 345mJ). Turn on the nanosecond pulse laser, emit a pulsed laser beam, and use the interference cutoff filter to divide the pulsed laser into pulsed laser beams with wavelengths of 1064nm and 532nm, respectively. The laser with a wavelength of 1064nm is reflected by a reflector, and then focused by a focusing mirror, through quartz glass, and directly acts on the surface of the graphite layer. The other laser with a wavelength of 532nm is reflected by a reflector, and then focused by a focusing mirror on the surface of the metal nanowire. With the three-coordinate mobile platform (moving speed is 0.1mm / s), an "S" type scanning path is used to complete the welding operation of the spatially staggered copper metal nanowires in the target area.
[0055] like Figure 2The figure shows the schematic diagram of the change of the position of the metal nanowires during the impact welding process. In this embodiment, the laser welding of the spatially staggered copper metal nanowires on the surface of the polyethylene terephthalate (PET) substrate is as follows: the reverse laser plasmon effect is used to locally heat the node area of the staggered metal nanowires, and the forward pulse laser is used to perform the impact operation, shorten the spacing of the spatially staggered nanowires, reduce the virtual overlap phenomenon, and enhance the heating effect. In the case that the metal nanowires are not melted as a whole, the original comprehensive mechanical properties of the metal nanowires are retained to the maximum extent, and the high reliability welding operation of the spatially staggered nanowires is achieved.
[0056] Finally, it should be noted that the above is only used to illustrate the technical solution of the present invention, rather than to limit it; although the present invention is described in detail with reference to the specific implementation methods, ordinary technicians in the field should understand that they can still modify the technical solutions recorded in the above-mentioned specific implementation methods, or replace some of the technical features therein with equivalents; and these modifications or replacements do not make the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the specific implementation methods of the present invention. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A metal nanowire impact welding method based on laser thermal coupling effect, It is characterized in that The steps include: Step S1. coating the surface of the constrained layer with metal nanowires, wherein the upper portion of the metal nanowires is provided with a constrained layer, an absorption layer and a protective layer in sequence from top to bottom; Step S2. Laying a protective layer material with a pre-set absorption layer on the surface above the metal nanowires; Step S3. Laying another constraining layer on top of the absorbing layer; Step S4. Turn on the laser to emit forward and reverse laser beams, wherein the laser emits a forward laser beam to perform a forward indirect impact operation on the metal nanowire; and at the same time, the laser emits a reverse laser beam to perform a reverse direct heating operation on the metal nanowire; and cooperates with a three-coordinate mobile platform to complete the welding operation of the metal nanowire; the time for the forward laser to irradiate the absorption layer and the time for the reverse laser to irradiate the metal nanowire can be adjusted by a time delay method, thereby controlling the sequence and duration of laser thermal regulation; the laser energy attenuation device can also be used to achieve the regulation of the laser beam intensity; the spot centers of the forward laser beam and the reverse laser beam coincide, thereby achieving an obvious thermal coupling effect in the beam interaction area; The online monitoring system is used to monitor the changes in the welding behavior of metal nanowires in real time.
2. The metal nanowire impact welding method based on laser thermal coupling effect according to claim 1, It is characterized in that In step S4, the metal nanowires in the target area can be gradually laser-shocked in a single-point stepping manner according to a fixed trajectory; the laser spot size and the number of spots can be adjusted by beam shaping or any method of a spatial light modulator to achieve single batch laser-shocked in the target area.
3. The metal nanowire impact welding method based on laser thermal coupling effect according to claim 1, It is characterized in that The forward laser beam directly irradiates the absorption layer to generate a plasma shock wave, which indirectly acts on the metal nanowires through the protective layer, and under the constraint of the constraint layers on both sides of the metal nanowires, punches the metal nanowires to shorten the distance between adjacent nanowires; the reverse laser beam irradiates the metal nanowires to achieve effective heating of the node area of adjacent metal nanowires, and the node area is an area with a diameter less than 1 micron with the center of the nanowire overlap point as the center.
4. The metal nanowire impact welding method based on laser thermal coupling effect according to claim 1, It is characterized in that The forward laser beam is a pulsed laser, and the reverse laser beam can be either a continuous laser or a pulsed laser.
5. The metal nanowire impact welding method based on laser thermal coupling effect according to claim 1, It is characterized in that The positive and negative laser beams can be generated separately by two lasers, or by one laser; the method of generating the positive and negative laser beams by one laser is: using any three or more optical path management elements among a beam expander, a beam splitter, a reflector or a focusing mirror to divide a single laser beam into two laser beams.
6. The metal nanowire impact welding method based on laser thermal coupling effect according to claim 1, It is characterized in that The constraint layer above the metal nanowires is any one of transparent ceramics, BK-7 glass or quartz glass; the constraint layer below the metal nanowires is any one of transparent ceramics, BK-7 glass, quartz glass or a flexible transparent substrate; the absorption layer is any one of graphite, black paint, black tape or a light-absorbing metal film; the protective layer is any one of pure metal or its alloy materials with a yield strength lower than 500 MPa.
Citation Information
Cited By
Device and method for manufacturing flexible transparent conductive film through roll-to-roll laser shock
CN120048586A
Device and method for roll-to-roll production of flexible transparent conductive film with protective layer