Method for reducing magnesium content in copper-cobalt hydrometallurgy cobalt slag

By using high-purity magnesium oxide fine powder and adding ammonium salt as a mixing aid in the copper-cobalt hydrometallurgical process, magnesium oxide slurry was prepared for room temperature wet leaching, which solved the problem of high magnesium content in cobalt slag, improved cobalt grade, reduced magnesium oxide usage, and lowered costs.

CN118910425APending Publication Date: 2024-11-08WESTERN MINING CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970096.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In existing technologies, when magnesium oxide is used in the cobalt precipitation process in copper-cobalt hydrometallurgical processes, the magnesium content in the cobalt slag is high, exceeding industry standards. This increases the cost of removing impurities from crude cobalt hydroxide, and the increased surface energy after fine grinding of magnesium oxide leads to agglomeration, affecting the cobalt grade.

Method used

High-purity magnesium oxide fine powder was used, and ammonium salt was added as a mixing agent to prepare magnesium oxide slurry. Cobalt was then leached by wet leaching at room temperature. The molar ratio of magnesium oxide to cobalt was controlled, and the product was obtained by filtration and drying to produce low-magnesium cobalt hydroxide.

Benefits of technology

It effectively reduced the magnesium content in cobalt slag, improved the cobalt grade, reduced the consumption of magnesium oxide, reduced the cost of impurity removal, and reduced the amount of magnesium oxide used by optimizing the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910425A_ABST
    Figure CN118910425A_ABST
Patent Text Reader

Abstract

The invention discloses a method for reducing the content of magnesium in copper-cobalt hydrometallurgy cobalt slag, which comprises the following steps: adding ammonium salt during magnesium oxide size mixing, so that magnesium oxide is hydrated in an aqueous solution containing the ammonium salt; then magnesium oxide slurry is added into the cobalt precipitation pre-solution for cobalt precipitation; and finally, carrying out solid-liquid separation to obtain coarse cobalt hydroxide with low magnesium content. The ammonium salt is used for promoting dispersion of magnesium oxide in the cobalt precipitation pre-solution, the content of impurity magnesium in the crude cobalt hydroxide is reduced, and the impurity removal cost of the crude cobalt hydroxide is further reduced. The application of magnesium oxide prepared by a salt lake chemical method in the field of cobalt precipitation is solved. Ammonium salt is selected as a mixing aid of magnesium oxide, the dosage is small, and the influence on the cobalt precipitation process is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical production, and in particular to a method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag. Background Art

[0002] The metallurgical process of copper-cobalt oxide ore mostly adopts a wet process. In the wet metallurgical process, the cobalt precipitation agent includes magnesium oxide, calcium oxide and liquid alkali. Since magnesium oxide provides mild alkalinity, the crude cobalt hydroxide obtained has a high grade and low water content, and has become the main cobalt precipitation agent. The preparation method of magnesium oxide is to calcine magnesium-rich ore or magnesium-containing inorganic salt or alkali. The magnesium-containing ore is mainly dolomite and magnesite. The calcination process will produce a large amount of CO2, which has a great impact on the environment. At the same time, the product contains a small amount of impurity ions such as Ca and Si. Magnesium-containing inorganic salts or alkalis include magnesium hydroxide, magnesium chloride, basic magnesium carbonate, etc. Since the highly corrosive gas HCl will be produced during the calcination of magnesium chloride, the requirements for the reaction device are very high. Basic magnesium carbonate will also produce CO2 after calcination. However, the process of calcining magnesium hydroxide to prepare magnesium oxide does not produce CO2, which is environmentally friendly.

[0003] The chemical synthesis of industrial magnesium hydroxide is obtained by co-precipitation of salt lake magnesium resources and ammonia. This process makes full use of the Qinghai salt lake magnesium resources. The product obtained has high purity but large particles. The magnesium oxide obtained by calcination is also large and needs to be finely ground before it can be used for cobalt precipitation. After fine grinding, the surface energy of the product magnesium oxide increases significantly, resulting in increased agglomeration during the cobalt precipitation process. The magnesium content in the cobalt slag after cobalt precipitation is about 10%, which reduces the cobalt grade in the cobalt slag and is lower than the industry standard secondary product requirements for crude cobalt hydroxide, increasing the consumption of reagents for further impurity removal of crude cobalt hydroxide. Therefore, solving the magnesium content of cobalt slag in the copper-cobalt hydrometallurgical process in the preparation of magnesium oxide by precipitation has important economic and social effects. Summary of the invention

[0004] In view of the defects of the prior art, the present invention provides a method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag, which has a simple process, can improve the cobalt grade, reduce the unit consumption of magnesium oxide, and has a lower cost.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solution: a method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag, characterized by: performing the following steps:

[0006] Step 1: Weigh high-purity magnesium oxide fine powder prepared by chemical method;

[0007] Step 2: preparing magnesium oxide slurry, and adding ammonium salt as a mixing aid during preparation;

[0008] Step 3: adding magnesium oxide slurry to the cobalt precipitation pre-liquid to carry out wet leaching of cobalt at room temperature to obtain crude cobalt hydroxide;

[0009] Step 4: The obtained crude cobalt hydroxide is filtered and dried to obtain a low-magnesium cobalt hydroxide product.

[0010] In step 2, the mixing aid is ammonium sulfate, ammonium chloride, ammonium bicarbonate or ammonium carbonate, the concentration of the mixing aid is 0.02-0.5 mol / L, more preferably 0.1-0.3 mol / L, the solid content (mass) of magnesium oxide is 5-30%, and the pretreatment time is 5-30 min.

[0011] In step 3, the magnesium oxide slurry is added to the cobalt precipitation pre-liquid for wet leaching of cobalt under the following control conditions: n(MgO):n(Co)=0.6-1.2:1 (molar ratio), no heating, stirring speed of 100-400 r / min, reaction time of 2-10 h.

[0012] In step 4, the crude cobalt hydroxide is filtered and dried to prepare a low-magnesium cobalt hydroxide product at a drying temperature of 60-80° C. The magnesium content can meet the standard first-class requirements of crude cobalt hydroxide, the cobalt recovery rate is above 80%, and the cobalt grade is above 45%.

[0013] Preferably, in step 2, the concentration of the auxiliary mixing agent is 0.1-0.3 mol / L, the solid content of magnesium oxide is 10%, and the pretreatment time is 10 min.

[0014] Preferably, the control conditions in step 3 are: n(MgO):n(Co)=0.6-0.8:1, and the reaction time is 4-6h.

[0015] In step 1, the high-purity magnesium oxide fine powder is obtained by coprecipitating magnesium hydroxide from salt lake bischofite, and then dynamically calcining and finely grinding to obtain a high-purity magnesium oxide fine powder, wherein the chlorine content is 0.5-0.6%. The magnesium oxide content is 95%-97%, and the particle size D 50 5-6μm, calcium oxide ≤0.05%, chloride 0.6%, disordered particles.

[0016] The cobalt content in the cobalt precipitation pre-liquid in step 3 is 1.0-12.0 g / L, the manganese content is 0.3-3.0 g / L, and the magnesium content is 0-3.5 g / L.

[0017] Since the surface energy of magnesium oxide prepared by the precipitation method increases after fine grinding, when it is directly used in the hydrometallurgical cobalt precipitation process, it will cause the magnesium content in the crude cobalt hydroxide to increase, exceeding the standard requirements and increasing the cost of removing impurities from the cobalt hydroxide. The present invention selects ammonium salt as a mixing aid in the process of magnesium oxide slurry preparation, and utilizes the ammonium salt to promote the hydration effect of magnesium oxide in water, thereby improving the dissolution efficiency of magnesium oxide, and further controls the magnesium content in the cobalt slag without extending the process flow, adding auxiliary equipment, and increasing the reaction temperature, thereby ensuring a relatively high level of cobalt grade; secondly, through the promoting effect of the mixing aid on the hydration of magnesium oxide in the cobalt precipitation system, the amount of the mixing aid is only 1 / 600 of the amount of magnesium oxide, and the amount is small; thirdly, due to the promoting effect of the mixing aid on the hydration of magnesium oxide, the ineffective amount of magnesium oxide generated by agglomeration in the cobalt precipitation system is reduced, so the unit consumption of magnesium oxide can be reduced by more than 30%, significantly reducing the cost; finally, since nickel and cobalt have similar chemical properties and are associated minerals, magnesium oxide is also used to recover nickel in the hydrometallurgical process, and the use of ammonium salt as a mixing aid to reduce the magnesium content of magnesium oxide in nickel slag is also applicable, thereby expanding the application field. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0019] The following is combined with Figure 1 The present invention is further described by specific embodiments:

[0020] Example 1

[0021] Weigh 1.17g of magnesium oxide, disperse it in 0.3mol / L, 20mL of ammonium chloride, prepare magnesium oxide slurry, magnesium oxide solid content 5%, pretreatment time 10min. Then add magnesium oxide slurry to cobalt precipitation pre-liquid for wet leaching of cobalt, cobalt precipitation pre-liquid 200mL, wherein the cobalt content is 10.7g / L, the manganese content is 2.34g / L, the magnesium content is 3.02g / L, the reaction is carried out at room temperature for 6h, the stirring speed is 400r / min, and the magnesium oxide unit consumption is 0.676t / tCo.

[0022] Results: The cobalt grade in the crude cobalt hydroxide was 45.30%, and the impurity magnesium content was 2.41%.

[0023] Example 2

[0024] Weigh 1.17g of magnesium oxide, disperse it in 0.1mol / L, 10mL of ammonium bicarbonate, prepare magnesium oxide slurry, magnesium oxide solid content 10%, pretreatment time 30min. Then add magnesium oxide slurry to cobalt precipitation pre-liquid for wet leaching of cobalt, cobalt precipitation pre-liquid 200mL, wherein the cobalt content is 1.7g / L, the manganese content is 0.34g / L, and the magnesium content is 0.02g / L, react at room temperature for 10h, stirring speed 300r / min.

[0025] Results: The cobalt grade in the crude cobalt hydroxide was 45.26%, the impurity magnesium content was 2.67%, and the unit consumption of magnesium oxide was 0.669t / t Co.

[0026] Example 3

[0027] Weigh 1.17g of magnesium oxide. Disperse magnesium oxide in 0.5mol / L, 3mL of ammonium sulfate to prepare magnesium oxide slurry with a magnesium oxide solid content of 30% and a pretreatment time of 2min. Then add magnesium oxide slurry to the cobalt precipitation pre-liquid for wet leaching of cobalt. The cobalt precipitation pre-liquid is 200mL, with a cobalt content of 11.7g / L, a manganese content of 2.94g / L, and a magnesium content of 3.42g / L. The reaction is carried out at room temperature for 2h and the stirring speed is 100r / min.

[0028] Results: The cobalt grade in the crude cobalt hydroxide was 47.24%, the impurity magnesium content was 1.47%, and the unit consumption of magnesium oxide was 0.632t / t Co.

[0029] Comparative Example

[0030] Weigh 1.17g of magnesium oxide. Disperse magnesium oxide in 10mL of water to prepare magnesium oxide slurry with a solid content of 10% and a pretreatment time of 5min. Then add magnesium oxide slurry to the cobalt precipitation pre-liquid for wet leaching of cobalt. The cobalt precipitation pre-liquid is 200mL, with a cobalt content of 11.7g / L, a manganese content of 2.94g / L, and a magnesium content of 3.42g / L. The reaction is carried out at room temperature for 2h and the stirring speed is 100r / min.

[0031] Results: The cobalt grade in the crude cobalt hydroxide was 34.73%, the impurity magnesium content was 10.18%, and the unit consumption of magnesium oxide was 0.95t / t Co.

[0032] The present invention has been described in detail above. The above description is only a preferred embodiment of the present invention and should not limit the scope of implementation of the present invention. That is, all equivalent changes and modifications made within the scope of this application should still fall within the scope of the present invention.

Claims

1. A method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag, Features: Follow these steps: Step 1: Weigh high-purity magnesium oxide fine powder prepared by chemical method; Step 2: preparing magnesium oxide slurry, and adding ammonium salt as a mixing aid during preparation; Step 3: adding magnesium oxide slurry to the cobalt precipitation pre-liquid to carry out wet leaching of cobalt at room temperature to obtain crude cobalt hydroxide; Step 4: Filter and dry the obtained crude cobalt hydroxide to obtain a low-magnesium cobalt hydroxide product.

2. The method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag according to claim 1, Features: In step 2, the mixing aid is ammonium sulfate, ammonium chloride, ammonium bicarbonate or ammonium carbonate, the concentration of the mixing aid is 0.02-0.5 mol / L, the solid content of magnesium oxide is 5-30%, and the pretreatment time is 5-30 min.

3. The method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag according to claim 1, Features: In step 3, the control conditions for adding magnesium oxide slurry to the cobalt precipitation pre-liquid for wet leaching of cobalt are: n(MgO):n(Co)=0.6-1.2:1, no heating, stirring speed 100-400r / min, reaction time 2-10h; the cobalt content in the cobalt precipitation pre-liquid is 1.0-12.0g / L, the manganese content is 0.3-3.0g / L, and the magnesium content is 0-3.5g / L.

4. The method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag according to claim 1, Features: In step 4, the crude cobalt hydroxide is filtered and dried to prepare a low-magnesium cobalt hydroxide product at a drying temperature of 60-80° C., a cobalt recovery rate of more than 80%, and a cobalt grade of more than 45%.

5. The method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag according to claim 2, Features: In step 2, the concentration of the auxiliary mixing agent is 0.1-0.3 mol / L, the solid content of magnesium oxide is 10%, and the pretreatment time is 10 minutes.

6. The method for reducing the magnesium content in copper-cobalt hydrometallurgical cobalt slag according to claim 3, Features: The control conditions in step 3 are: n(MgO):n(Co)=0.6-0.8:1, and the reaction time is 4-6h.

7. The method for reducing the magnesium content in the copper-cobalt hydrometallurgical cobalt slag according to claim 1, 3 or 6, Features: In step 1, the high-purity magnesium oxide fine powder is obtained by co-precipitating magnesium hydroxide based on salt lake bischofite, and then dynamically calcining and finely grinding the high-purity magnesium oxide fine powder, wherein the chlorine content is 0.5-0.6%.