Sintering method for improving ore-forming rate of laterite-nickel ore sintered ore
By using low-nickel ore mixing and boric acid additives in laterite nickel ore sintering, combined with ignition sintering technology, the alkalinity of sintering ore is controlled, the powdering problem caused by calcium orthosilicate is solved, the mineralization rate and sintering strength are improved, and the mineralization rate and sintering strength are achieved. An efficient sintering process.
Patent Information
- Application Number
- CN202411079964.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing laterite nickel ore sintering technology, calcium silicate additives will lead to sintering ore pulverization during use, affecting the ore formation rate, and the sintering ore strength and smelting performance are poor.
The mixture of four nickel ores mainly consists of low nickel ores is adopted to control the particle size and proportion of nickel ores, and add about 0.05% boric acid additive to the mixture. Through ignition and sintering technology, the alkalinity of the sintered ores is controlled between 1.25-1.40 In between, boric acid-containing catalytic fixation carbon is used to reduce the ignition point of the fuel and increase the sintering speed and strength.
It effectively improves the quality and mineralization rate of the sintered ore, inhibits the natural powderization of the sintered ore, reduces the melting temperature of the nickel ore, shortens the sintering time, improves the combustion speed and the utilization coefficient of the sintering machine, and improves the smelting performance.
Smart Images

Figure CN118910426A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of laterite nickel ore sintering, and in particular to a sintering method for improving the mineralization rate of laterite nickel ore sintering. Background Art
[0002] Laterite nickel ore is usually an important nickel ore resource. Laterite nickel ore is an enrichment of nickel in oxidizing soils such as laterite or brown soil. Laterite nickel ore is a clay-like ore formed by long-term weathering, leaching and sedimentation of nickel oxide deposits. Laterite nickel ore is mainly composed of limonite layer, transition layer and humus layer. Laterite nickel ore usually needs to be sintered by nickel ore.
[0003] Laterite nickel ore sintering generally refers to a process in which nickel ore, fuel, solvent and other auxiliary materials are mixed with water and ignited and ventilated. The laterite nickel ore sintering in the prior art generally adopts a high temperature method to make the laterite nickel ore produce a large amount of liquid phase, and then the powder ore is bonded into blocks to complete the sintering of the laterite nickel ore.
[0004] However, this method may cause the quality of the binding phase to affect the strength and smelting performance of the sintered ore. In order to improve this situation, calcium orthosilicate additives are used. However, calcium orthosilicate additives will undergo phase changes during use, causing the pulverization of the sintered ore, affecting the mineralization rate of the laterite nickel ore sintering ore, and making it inconvenient to sinter the laterite nickel ore. Summary of the invention
[0005] The object of the present invention is to provide a sintering method for improving the sintering rate of laterite nickel ore, so as to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a sintering method for improving the sintering rate of laterite nickel ore, comprising the following specific steps: Step 1: Select laterite nickel ore sintering raw materials, mainly low-nickel ore, and then select by mixing 4 kinds of nickel ores, and control the nickel ore particle size and proportion of the 4 kinds of nickel ores; Step 2: Mixing the laterite nickel ore sintering raw materials, using a mixing device to mix the laterite nickel ore sintering raw materials to obtain a mixed material; Step 3: Adding additives and water, by setting up a separate feeding bin and feeder, adding the boric acid additive at a ratio of 0.05% to the mixture of step 2 using a conveyor belt, and then adding an appropriate amount of water to the mixing equipment to fully mix the mixture and granulate it, and then obtain the mixture, which must meet the nickel ore particle size requirements; Step 4: Ignite and sinter the mixture. The mixture in step 3 is spread on a trolley with a base material thickness of 5 cm in a layer of 940 mm to keep the material surface flat. Then, an igniter is used to make the sintering machine and the fan cooperate to ignite and sinter the mixture, while controlling the composition of the sintered ore. Step 5: Obtain the ignition and sintering finished product.
[0007] Preferably, the particle sizes of the four types of nickel ores in step one are controlled to be >3 mm, 3-8 mm, 8-20 mm and <20 mm, respectively, and the particle sizes of the four types of nickel ores in step one account for 30%±5%, 60%±5%, 10%±3% and <1%, respectively.
[0008] Preferably, the mixing equipment in step 2 is a mixer, which includes a first roller and a second roller, the inclination angle of the first roller and the second roller is 3 degrees, and the rollers run at a speed of 45 Hz. At the same time, 13-15 cubic meters / hour of water is added to the mixture in step 2 in the first roller, and the mixing time of the mixture in the first roller and the second roller is 5 minutes.
[0009] Preferably, the particle size of the nickel ore mixture in step three meets the requirements of >3 mm, 3-8 mm, 8-20 mm and <20 mm, respectively, and the particle size proportion of the mixture in step three meets the requirements of 25%±3%, 65%±5%, 10%±2% and <0.5%, respectively.
[0010] Preferably, the dosage of the boric acid additive in step three is controlled to be 0.05% to 0.1%, and the moisture content of the mixture in step three is controlled to be less than 17.5%.
[0011] Preferably, the ignition temperature of the igniter in step 4 is 1150±20 degrees Celsius, the sintering frequency of the sintering machine is 20±0.5, and the tail temperature of the sintering machine is required to be <500 degrees Celsius.
[0012] Preferably, the sintered ore composition control in step 4 includes sintered ore basicity control, and the sintered ore basicity is controlled to be 1.25-1.40.
[0013] Preferably, the effective area of the trolley in step 4 is 150 square meters, and the size of the trolley is 3*1*1 meter, and the operating frequency of the trolley is 21.5-22 Hz.
[0014] Technical effects and advantages of the present invention: (1) The present invention uses a boron-containing additive to add a certain amount of boron-containing substances to the laterite nickel ore mixture, and the addition of boric acid additives reduces the generation temperature of the liquid phase during the sintering process, accelerates the sintering speed, shortens the sintering time, accelerates the sintering combustion speed, effectively catalyzes the fixed carbon to reduce the ignition point of the fuel, and is beneficial to the sintering operation of the laterite nickel ore, improves the quality of the sintered ore, and inhibits the natural pulverization of the sintered ore. At the same time, it is beneficial to reduce the melting temperature of the nickel ore, accelerate the liquid phase production speed, complete rapid bonding, thereby increasing the combustion speed and improving the utilization coefficient of the sintering machine; (2) The present invention selects nickel ore raw materials according to the particle size requirements, and controls the dosage of additives and the basicity of sintered ore, which is beneficial to improving the quality of the binding phase, so as to improve the poor strength of the sintered ore, the low yield rate and the low smelting performance. At the same time, it is beneficial to the cost control range to more effectively highlight the performance and role of the additives. At the same time, the basicity control is beneficial to improving the mineralization rate of laterite nickel ore sintered ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The figure is a schematic diagram of the sintering process of laterite nickel ore of the present invention. DETAILED DESCRIPTION
[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] Embodiment 1 like Figure 1 A sintering method for improving the mineralization rate of laterite nickel ore sintering is shown, including selecting laterite nickel ore sintering raw materials, selecting low-nickel ore as the main ore, and then selecting by mixing 4 kinds of nickel ores, and controlling the nickel ore particle size and proportion of the 4 kinds of nickel ores, the particle size of the 4 kinds of nickel ores are controlled to be >3 mm, 3-8 mm, 8-20 mm and <20 mm, respectively, the particle size proportions of the 4 kinds of nickel ores are 30%±5%, 60%±5%, 10%±3% and <1%, respectively, and the mixed composition of the 4 kinds of nickel ores is shown in the figure below: Mix the laterite nickel ore sintering raw materials, use a mixing device to mix the laterite nickel ore sintering raw materials, the mixing device is a mixer, the mixer includes a first roller and a second roller, the inclination angle of the first roller and the second roller is 3 degrees, and the rollers are operated at a speed of 45 Hz, and at the same time, the mixture in step 2 is added with water for 13 to 15 cubic meters per hour in the first roller, and the mixing time of the mixture in the first roller and the second roller is 5 minutes, thereby obtaining a mixture.
[0018] Addition of additives and water, by setting up a separate feeding bin and feeder, the boric acid additive is uniformly added to the mixture of step 2 using a conveyor belt at a ratio of 0.05%, and then an appropriate amount of water is added to the mixing equipment, the amount of boric acid additive is controlled to be 0.05% to 0.1%, and the moisture content of the mixture is controlled to be <17.5%, so that the mixture is fully mixed and granulated, and then a mixture is obtained. The mixture must meet the nickel ore particle size requirements. The nickel ore particle size requirements of the mixture are >3 mm, 3 ~8mm, 8~20mm and <20mm, the proportion of mixed material particle size meeting the requirements is 25%±3%, 65%±5%, 10%±2% and <0.5% respectively. In the use of boric acid additives to prevent sintering ore from pulverization and improve the mechanical and metallurgical properties of sintered ore, for laterite nickel ore, the dosage of additives is controlled within a certain range, so that the additives are beneficial to improve the various properties of nickel ore sintering. At the same time, the additive range can more effectively highlight the performance and function, and at the same time, it has The supporting process operation parameters include the moisture control range of the mixture <17.5%, the height of the sintering material layer 930-940 mm, and the key parameter is the alkalinity of the sintered ore. In the smelting of laterite nickel ore, the blast furnace requires a higher alkalinity, which is beneficial to the temperature in the furnace and the addition of fuel. However, after production verification, the mineralization rate of the sintered ore decreases under high alkalinity, and the pulverization rate also increases. Combining the two conditions, the alkalinity range is controlled at 1.25-1.40, which is beneficial to improve the mineralization rate of laterite nickel ore. Adding a certain amount of boron-containing substances to the mixture is beneficial to improving the quality of sintered ore and inhibiting the natural pulverization of sintered ore. Adding 0.03% to 0.1% boric acid additives to the mixture, the sintering ore return rate has a 1.5% to 2% reduction effect when using 0.03% boron-containing additives. With the increase of the amount of boron-containing additives added, the pulverization of the sintered ore is reduced and the return rate continues to decrease. When the addition amount reaches 0.1%, the return rate of the sintered ore decreases by 4% to 5%. At the same time, the effect on the cold strength of the sintered ore is compared with the sintering ore without additives and with 0.Based on the actual production data of 0.05% additive, under the same raw material conditions such as ore type, fuel, material layer, batch, air volume and water addition, the conversion strength is increased from 48% to 50% to 53% to 56%, which effectively improves the cold strength of sintered ore. The addition of boric acid reduces the generation temperature of liquid phase during sintering, accelerates the sintering speed, shortens the sintering time, and accelerates the sintering combustion speed. The melting speed of nickel ore during sintering is one of the decisive factors for the overall combustion speed. The additive can effectively catalyze the fixed carbon to reduce the ignition point of the fuel, and is conducive to reducing the melting temperature of nickel ore, so that the liquid phase production speed is accelerated, and the rapid bonding is completed, thereby increasing the combustion speed and improving the utilization coefficient of the sintering machine. From the actual production, the finished sintered ore before and after the use of the additive has also changed significantly. First of all, in terms of bonding mode, the liquid phase is generated more quickly and stably, and the bonding phase of the sintered ore is more stable. Different from the granular and incompletely melted mixed material particles that always appear before use, the surface of the finished sintered ore is bonded. After use, both the porosity and the bonding phase are significantly improved. .
[0019] The mixture is ignited and sintered, and the mixture in step 3 is spread on a trolley with a base material thickness of 5 cm in a layer of 940 mm. The effective area of the trolley is 150 square meters, and the size of the trolley is 3*1*1 meter. The operating frequency of the trolley is 21.5-22 Hz, so that the material surface remains flat. Then, an igniter is used to make the sintering machine and the fan cooperate to ignite and sinter the mixture. The sintering machine is a main equipment in a large-scale ferrous metallurgical sintering plant. The sintering machine is a key equipment in the exhaust sintering process. The sintering machine can sinter raw materials such as concentrate powder and rich ore powder of different compositions and different particle sizes into blocks, and partially eliminate harmful impurities such as sulfur and phosphorus contained in the ore. In this process, the raw materials are sintered at high temperature. After physical and chemical changes, sintered ore with certain strength and metallurgical properties is formed, which is beneficial to the sintering production of laterite nickel ore using nickel ore. The ignition temperature of the igniter is 1150±20 degrees Celsius. Taking 315 time / hour batch and 150 square meters sintering machine as an example, the fan air volume is controlled at about 600,000 cubic meters / hour, the sintering frequency of the sintering machine is 20±0.5, and the tail temperature of the sintering machine is required to be <500 degrees Celsius. At the same time, the sintered ore composition is controlled. The sintered ore composition control includes the sintered ore alkalinity control. Alkalinity control is beneficial in production. High alkalinity means a higher CaO content. This condition is more conducive to the formation of calcium silicate 2CaO+SiO2>Ca2SiO4. In the SiO2 content In the sintering of laterite nickel ore with a content of 5.8-6.2, the alkalinity control range of <1.4 can effectively reduce the return rate of ore. The alkalinity of the sintering frame is controlled at 1.25-1.40. After normal ignition, the boric acid additive has a lowering effect on the ignition point of carbon during the sintering process. The ignition temperature can be appropriately reduced by 20°C during the production process. Since the boric acid additive has the effect of increasing the combustion speed and reducing the melting temperature of the sintered ore, the wind should be reasonably used to control the opening of the fan and the damper, and the opening of the front and rear wind box dampers should be appropriately adjusted during the sintering process to avoid over-pumping of the sintered ore or rapid cooling of the upper sintered ore during the sintering process, so as to avoid the adverse effects on the sintering mineralization rate. The sintered ore has an effective area of 175 square meters. The cooling process on the 2.8*1.8*2.1m ring cooler should not be cooled too fast. The air door opening of the front-end cooling fan should be appropriately reduced. The air door opening of the No. 1 ring cooling fan is 50%-70%, the air door opening of the No. 2 ring cooling fan is 80%-99%, and the air door opening of the No. 3 ring cooling fan is 99%. The air door opening of the No. 4 ring cooling fan can be measured according to the sintering temperature at the 5 trolleys before the discharge port. The ore temperature may be controlled at 70-100 degrees Celsius, and the No. 4 ring cooling fan can be closed. If it is above 100 degrees Celsius, the appropriate air door opening can be adjusted according to the measured temperature. At the same time, this operation mode is conducive to suppressing the pulverization of the sintered ore and obtaining the ignition sintering product. The sintered ore composition control is shown in the following figure: Among them, the control of binary alkalinity index plays a key role in improving the mineralization rate. According to actual production data, the content of silicon dioxide in the sintering of Si02 laterite nickel ore does not change much, and its range is basically 5.8-6.3. Therefore, the control of quicklime is more critical. In this process, the proportion of lime in the mixture is 3.3%-3.9%. When the alkalinity of the finished sintered ore reaches above 1.4, the return rate is 1.0%-1.5% higher than that of the alkalinity of about 1.30. Therefore, alkalinity control is beneficial to improving the mineralization rate of laterite nickel ore sintered ore.
[0020] Embodiment 2 The laterite nickel ore sintering raw materials are selected by mixing and matching a variety of nickel ores.
[0021] The laterite nickel ore sintering raw materials are mixed, and a mixing device is used to mix the laterite nickel ore sintering raw materials to obtain a mixed material.
[0022] Additives and water are added and mixed by adding calcium orthosilicate additive.
[0023] The mixture is ignited and sintered. The mixture in step three is spread on a trolley to keep the material surface flat. Then an igniter is used to coordinate the sintering machine and the fan to ignite and sinter the mixture.
[0024] Obtain the ignition sintering finished product.
[0025] Embodiment 2 The laterite nickel ore sintering raw materials are selected by mixing and matching a variety of nickel ores.
[0026] The laterite nickel ore sintering raw materials are mixed, and a mixing device is used to mix the laterite nickel ore sintering raw materials to obtain a mixed material.
[0027] Additives and water are added and mixed by adding calcium orthosilicate additive.
[0028] The mixture is ignited and sintered. The mixture in step three is spread on a trolley to keep the material surface flat. Then an igniter is used to coordinate the sintering machine and the fan to ignite and sinter the mixture.
[0029] Obtain the ignition sintering finished product.
[0030] The difference between Example 2 and Example 1 is that the selection of nickel ore is not controlled, calcium orthosilicate additive is used for mixing, and the sintering basicity is not controlled.
[0031] Embodiment 3 Select laterite nickel ore sintering raw materials, mainly select low-nickel ore, and then select by mixing 4 kinds of nickel ores, and control the nickel ore particle size and proportion of the 4 kinds of nickel ores.
[0032] The laterite nickel ore sintering raw materials are mixed, and a mixing device is used to mix the laterite nickel ore sintering raw materials to obtain a mixed material.
[0033] Additives and water are added and mixed by adding calcium orthosilicate additive.
[0034] The mixture is ignited and sintered. The mixture in step three is spread on a trolley to keep the material surface flat. Then an igniter is used to coordinate the sintering machine and the fan to ignite and sinter the mixture.
[0035] Obtain the ignition sintering finished product.
[0036] The difference between Example 3 and Example 1 is that calcium orthosilicate additive is used for mixing and the sintering basicity is not controlled.
[0037] Embodiment 4 The laterite nickel ore sintering raw materials are selected by mixing and matching a variety of nickel ores.
[0038] The laterite nickel ore sintering raw materials are mixed, and a mixing device is used to mix the laterite nickel ore sintering raw materials to obtain a mixed material.
[0039] Additives and water are added by setting up a separate feeding bin and feeder, and the boric acid additive is evenly added to the mixture of step 2 at a ratio of 0.05% using a conveyor belt, and then a proper amount of water is added to the mixing equipment to fully mix the mixture and granulate it to obtain a mixture. The mixture must meet the nickel ore particle size requirements.
[0040] The mixture is ignited and sintered. The mixture in step three is spread on a trolley to keep the material surface flat. Then an igniter is used to coordinate the sintering machine and the fan to ignite and sinter the mixture.
[0041] Obtain the ignition sintering finished product.
[0042] The difference between Example 4 and Example 1 is that the selection of nickel ore is not controlled and the sintering basicity is not controlled.
[0043] Embodiment 5 The laterite nickel ore sintering raw materials are selected by mixing and matching a variety of nickel ores.
[0044] The laterite nickel ore sintering raw materials are mixed, and a mixing device is used to mix the laterite nickel ore sintering raw materials to obtain a mixed material.
[0045] Additives and water are added and mixed by adding calcium orthosilicate additive.
[0046] The mixture is ignited and sintered. The mixture in step 3 is spread on a trolley with a base material thickness of 5 cm in a layer of 940 mm to keep the material surface flat. Then an igniter is used to coordinate the sintering machine and the fan to ignite and sinter the mixture, while controlling the composition of the sintered ore.
[0047] Obtain the ignition sintering finished product.
[0048] The difference between Example 5 and Example 1 is that the selection of nickel ore is not controlled, and calcium orthosilicate additive is used for mixing.
[0049] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A sintering method for improving the sintering rate of laterite nickel ore, characterized in that: The specific steps include: Step 1: Select laterite nickel ore sintering raw materials, mainly low-nickel ore, and then select by mixing 4 kinds of nickel ores, and control the nickel ore particle size and proportion of the 4 kinds of nickel ores; Step 2: Mixing the laterite nickel ore sintering raw materials, using a mixing device to mix the laterite nickel ore sintering raw materials to obtain a mixed material; Step 3: Adding additives and water, by setting up a separate feeding bin and feeder, adding the boric acid additive at a ratio of 0.05% to the mixture of step 2 using a conveyor belt, and then adding an appropriate amount of water to the mixing equipment to fully mix the mixture and granulate it, and then obtain the mixture, which must meet the nickel ore particle size requirements; Step 4: Ignite and sinter the mixture. The mixture in step 3 is spread on a trolley with a base material thickness of 5 cm in a layer of 940 mm to keep the material surface flat. Then, an igniter is used to make the sintering machine and the fan cooperate to ignite and sinter the mixture, while controlling the composition of the sintered ore. Step 5: Obtain the ignition and sintering finished product.
2. A sintering method for improving the sintering rate of laterite nickel ore according to claim 1, characterized in that: The controlled particle sizes of the four types of nickel ores in the step one are respectively >3 mm, 3-8 mm, 8-20 mm and <20 mm, and the proportions of the four types of nickel ores in the step one are respectively 30%±5%, 60%±5%, 10%±3% and <1%.
3. A sintering method for improving the sintering rate of laterite nickel ore according to claim 1, characterized in that: The mixing equipment in step 2 is a mixer, which includes a first roller and a second roller. The inclination angle of the first roller and the second roller is 3 degrees, and the rollers run at a speed of 45 Hz. At the same time, 13 to 15 cubic meters of water are added to the mixture in step 2 in the first roller per hour, and the mixing time of the mixture in the first roller and the second roller is 5 minutes.
4. A sintering method for improving the sintering rate of laterite nickel ore according to claim 1, characterized in that: The particle size of the nickel ore mixture in the step three meets the requirements of >3 mm, 3-8 mm, 8-20 mm and <20 mm, respectively, and the particle size proportion of the mixture in the step three meets the requirements of 25%±3%, 65%±5%, 10%±2% and <0.5%, respectively.
5. The sintering method for improving the sintering rate of laterite nickel ore according to claim 1, characterized in that: The dosage of the boric acid additive in step three is controlled to be 0.05% to 0.1%, and the moisture content of the mixture in step three is controlled to be less than 17.5%.
6. The sintering method for improving the sintering rate of laterite nickel ore according to claim 1, characterized in that: The ignition temperature of the igniter in step 4 is 1150±20 degrees Celsius, the sintering frequency of the sintering machine is 20±0.5, and the tail temperature of the sintering machine is required to be <500 degrees Celsius.
7. The sintering method for improving the sintering rate of laterite nickel ore according to claim 1, characterized in that: The sintered ore composition control in step 4 includes sintered ore basicity control, and the sintered ore basicity is controlled to be 1.25-1.