Hard alloy with needle-like tissue and preparation method thereof

The WC-VC-Co composite powder is prepared by ball milling and spray granulation technology, combined with selected laser melting and heat treatment, and the problem of difficult to prepare complex shapes and special crystal oriented cemented carbides in the prior art is solved, and the needle-like structure and High-performance cemented carbide parts preparation simplifies process and improves performance.

CN118910451AActive Publication Date: 2024-11-08BEIJING UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410969351.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The prior art is difficult to prepare cemented carbide parts with complex geometric shapes and special crystal orientations. The traditional method has harsh process conditions and is difficult to prepare, which limits its practical application.

Method used

The WC-VC-Co composite powder was prepared by ball mill, and high-density powder was formed by spray granulation and heat treatment. The WC and V4WC5 phases were used to form metastable VWC2 phases during melting and solidification, and then heat treatment was used to make them. It is decomposed into WC and V4WC5, which promotes the orientation growth of WC grains and forms cemented carbide with needle-like tissue.

Benefits of technology

The preparation of cemented carbide parts with free needle-like structure and shape is realized, the process flow is simplified, and the hardness and wear resistance of cemented carbide is improved, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004952687750000011
    Figure HDA0004952687750000011
  • Figure HDA0004952687750000021
    Figure HDA0004952687750000021
  • Figure HDA0004952687750000031
    Figure HDA0004952687750000031
Patent Text Reader

Abstract

The invention discloses a hard alloy with a needle-like structure and a preparation method thereof, and belongs to the technical field of hard alloy additive manufacturing. Comprising the following steps: preparing WC-VC-Co spherical composite powder by adopting WC powder, Co powder and VC powder with the average particle size of less than 1 mu m as raw materials; carrying out heat treatment and size grading, and then carrying out printing forming by adopting powder spreading type selective laser melting equipment, so that WC and VC form a VWC2 phase in situ under the action of laser; and the hard alloy part obtained through printing is subjected to heat treatment for 50-80 min in the argon atmosphere with the temperature ranging from 1410 DEG C to 1480 DEG C and the pressure ranging from 5 MPa to 6 MPa, so that the VWC2 phase is decomposed into WC and V4WC5, and oriented growth of the formed WC is promoted. The prepared hard alloy with the needle-shaped structure is compact in microstructure, needle-shaped WC is evenly distributed in different spatial directions, and the volume content of the needle-shaped structure is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of cemented carbide additive manufacturing, and specifically relates to a process method for preparing a cemented carbide with a needle-like structure by using laser 3D printing and subsequent heat treatment. Technical Background

[0002] Cemented carbide represented by WC-Co composition has high hardness, strength and wear resistance, and its Vickers hardness can reach 1000~2400kgf / mm 2 The bending strength can reach more than 5000MPa, and it can maintain excellent comprehensive mechanical properties even in high temperature and high pressure environments. This makes cemented carbide widely used in many industrial fields by being processed into metal cutting tools, molds and wear-resistant parts.

[0003] Due to the difficulty of subsequent mechanical processing of cemented carbide, powder metallurgy process is currently the main preparation method for its various products. The cemented carbide prepared by this process is generally composed of equiaxed carbide (including WC, TiC, NbC, etc.) grains to form a skeleton in terms of microstructure, and the skeleton gap is filled with metals such as Co, Ni, Fe or their alloys. The carbide in this metal-ceramic composite material mainly provides high hardness and wear resistance for the alloy, while the metal bonding phase provides plastic toughness, coordinates plastic deformation when the alloy is subjected to external loads, relieves stress concentration, thereby delaying fracture and improving the strength of cemented carbide.

[0004] Studies have found that by using a specific preparation process, WC grains with a close-packed hexagonal structure can be preferentially grown in a direction perpendicular to their prism or basal plane, forming a plate-like or lath-like morphology. Since the basal plane and prism of WC have different hardness and wear resistance, this kind of cemented carbide with a special orientation has obvious anisotropy in performance. By utilizing this, the prepared cemented carbide products can have more outstanding performance in certain application scenarios, maximizing their advantages. However, the preparation of the above-mentioned cemented carbide with a special orientation often requires harsh process conditions, such as high-energy ball milling and filtration to make the initial powder oriented and distributed; applying unidirectional pressure based on special sintering equipment to make WC grains grow in an oriented manner, etc. Due to the difficulty of preparation, the practical application of such cemented carbide is limited. In particular, it is difficult to prepare cemented carbide parts with complex geometric shapes and special crystal orientations by traditional methods.

[0005] In view of the above problems, the present invention proposes a method for preparing cemented carbide with needle-like structure based on innovative design of composition and regulation of laser 3D printing process, which realizes the free design of the shape of cemented carbide parts with special crystal orientation for the first time. Summary of the invention

[0006] The preparation process and principle provided by the present invention are as follows: firstly, WC-VC-Co composite powder with uniform dispersion of each phase is obtained by ball milling, then spray granulation and heat treatment are performed to obtain printable powder with high density, during which a certain amount of WC and VC react to form V4WC5 phase; selective laser melting equipment is used to print the powder, so that the remaining WC and V4WC5 phases in the powder react in situ to form metastable VWC2 phase during the melting and extremely rapid solidification of the powder; then, heat treatment is performed to improve the density of the printed part, at which time a part of the metastable VWC2 phase is decomposed into WC and V4WC5 phases again, and due to the aggregation and distribution of V atoms on the special crystal plane of the WC grains in this process, oriented growth occurs, thereby obtaining a new type of WC-Co cemented carbide with a needle-like structure.

[0007] The present invention provides a cemented carbide with needle-like structure and a preparation method thereof, characterized in that the method comprises the following steps:

[0008] (1) Using WC, Co and VC powders with an average particle size of less than 1 μm as raw materials, the WC-VC-Co composite powder is prepared so that the mass fraction of VC is 5%-22% and the mass fraction of Co is 10%-20%, and the mixture is fully wet-milled with anhydrous ethanol as the medium to ensure that the three raw material powders are evenly mixed before drying. The dried powder is mixed with deionized water and polyethylene glycol to form a slurry, and agglomerated and granulated by a high-speed centrifugal atomization drying process to obtain a WC-VC-Co spherical composite powder;

[0009] (2) The spherical composite powder obtained in the above steps is heat treated to remove polyethylene glycol while allowing the agglomerated particles to obtain a certain cohesive strength, high density and fluidity, and at the same time, part of WC and VC react to form V4WC5 phase. The heat treatment temperature is 1180-1250°C, and the holding time is 90-120 minutes; then, the particles with too large and too small particle sizes in the heat-treated powder are removed by airflow classification to obtain the WC-V4WC5-Co spherical composite powder with a particle size distribution of 10-30μm required for printing;

[0010] (3) Using the powder classified in the above steps as raw material, a powder spreading type selective laser melting device is used for printing and forming, so that WC and V4WC5 form VWC2 phase in situ under the action of laser. The laser printing process parameters used are: laser power 100-140W, scanning rate 800-1000mm / s, scanning spacing 0.04mm, and powder spreading layer thickness 0.03mm.

[0011] (4) The printed parts are subjected to atmosphere protection heat treatment at a temperature of 1410-1480°C. When the temperature rises to the target temperature, 5-6 MPa of argon gas is introduced and kept at this pressure for 50-80 min to decompose the VWC2 phase into WC and V4WC5, and to promote the oriented growth of the formed WC. After cooling to room temperature, a cemented carbide part with a needle-like structure and freely designable shape is obtained.

[0012] In the further step (3), the phases of the parts formed by the powder under the action of laser include: VWC2 and relatively small amounts of WC, W2C, Co3W3C.

[0013] In the further step (4), the phases of the parts after heat treatment include: WC, V4WC5, VWC2 and Co.

[0014] Furthermore, the volume content of the needle-like structure in the part is finally obtained to be 40%-70%, the average length of the needle-like WC grains is 1.0-2.2μm, and the average diameter ranges from 0.1-0.3μm.

[0015] The technical features and advantages of the method of the present invention are mainly as follows: (1) The present invention introduces an appropriate amount of VC into traditional WC-Co powder, and then combines it with a selective laser melting process to realize the preparation of cemented carbide parts with needle-like structure and freely designable shape. The method is simple and easy to implement, and has great prospects for industrial application; (2) The present invention cleverly utilizes the metastable VWC2 phase, through its in-situ formation under the action of laser and its decomposition during the heat treatment process, so that V atoms are segregated at a special WC / Co interface, thereby realizing the oriented growth of the WC phase under conventional heat treatment process conditions, and obtaining WC grains with a one-dimensional needle-like structure. Compared with the lath-like WC obtained by the traditional process, the aspect ratio of the needle-like WC grains (which can reach more than 7) is significantly increased; (3) The cemented carbide with needle-like structure prepared by the present invention has a dense microstructure, and the needle-like WC is evenly distributed in different directions in space, so that it has high hardness and excellent wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The scanning electron microscope morphology and particle size distribution of the spherical WC-VC-Co composite powder prepared by the present invention; wherein (a) is the scanning electron microscope morphology and particle size distribution of WC-5VC-12Co powder, (b) is the scanning electron microscope morphology and particle size distribution of WC-10VC-12Co powder, and (c) is the scanning electron microscope morphology and particle size distribution of WC-15VC-12Co powder;

[0017] Figure 2Phase analysis results of WC-V4WC5-Co spherical composite powder prepared by the present invention, and cemented carbide parts in laser-printed state and after heat treatment; wherein (a) is the phase composition of spherical composite powder, (b) is the phase composition of laser-printed cemented carbide, and (c) is the phase composition of cemented carbide after laser printing and heat treatment.

[0018] Figure 3 The figures are the microstructures of the cemented carbide samples after laser printing and 1410°C heat treatment observed under a scanning electron microscope of the present invention; wherein, (a) is the microstructure of the WC-5VC-12Co sample after laser printing and 1410°C heat treatment, (b) is the microstructure of the WC-10VC-12Co sample after laser printing and 1410°C heat treatment, and (c) is the microstructure of the WC-15VC-12Co sample after laser printing and 1410°C heat treatment. DETAILED DESCRIPTION

[0019] The present invention is further described below with reference to Example 1, Example 2 and Example 3, but the present invention is not limited to the following examples.

[0020] Example 1

[0021] WC, Co and VC powders with an average particle size of less than 1 μm are used as raw materials. The mass fraction of VC in the obtained WC-VC-Co composite powder is 5%, and the mass fraction of Co is 12%. The powder is fully wet-milled with anhydrous ethanol as the medium to ensure that the three raw material powders are evenly mixed before drying. The dried powder is mixed with deionized water and polyethylene glycol in proportion to form a slurry, and agglomerated and granulated by a high-speed centrifugal atomization drying process to obtain WC-VC-Co spherical composite powder. The spherical composite powder obtained in the above steps is heat-treated to remove polyethylene glycol while allowing the agglomerated particles to obtain a certain cohesive strength, high density and fluidity, and at the same time, part of WC and VC react to form V4WC5 phase. The heat treatment temperature is 1250°C, and the insulation time is 90 minutes. Then, the particles with too large and too small particle sizes in the heat-treated powder are removed by airflow classification to obtain the WC-V4WC5-Co spherical composite powder with a particle size distribution of 10-30 μm required for printing. Its morphology is as follows Figure 1 (a) Phase detection results are as follows Figure 2 (a) As shown. The powder after classification in the above steps is used as raw material, and the powder spreading type selective laser melting equipment is used for printing and forming, so that WC and V4WC5 form VWC2 phase in situ under the action of laser. The laser printing process parameters used are: laser power 100W, scanning rate 800mm / s, scanning spacing 0.04mm, and powder layer thickness 0.03mm. The phase detection results of laser printed cemented carbide are shown in Figure 2(b) As shown. The printed parts were subjected to atmosphere protection heat treatment at a temperature of 1410°C. When the temperature reached the target temperature, 5MPa of argon was introduced and kept at this pressure for 50 minutes to decompose the VWC2 phase into WC and V4WC5, and to promote the oriented growth of the formed WC. After cooling to room temperature, a cemented carbide part with a needle-like structure and freely designable shape was obtained. Figure 2 (c) and Figure 3 (a) shows the phase detection results of cemented carbide after laser printing and heat treatment, and the microstructure of cemented carbide with needle-like structure, in which the volume content of needle-like structure is about 40.59%, the average length of needle-like WC phase is 1.02μm, and the diameter is 0.13μm.

[0022] Example 2

[0023] WC, Co and VC powders with an average particle size of less than 1 μm are used as raw materials. The mass fraction of VC in the obtained WC-VC-Co composite powder is 10%, and the mass fraction of Co is 12%. The powder is fully wet-milled with anhydrous ethanol as the medium to ensure that the three raw material powders are evenly mixed before drying. The dried powder is mixed with deionized water and polyethylene glycol in proportion to form a slurry, and agglomerated and granulated by a high-speed centrifugal atomization drying process to obtain WC-VC-Co spherical composite powder. The spherical composite powder obtained in the above steps is heat-treated to remove polyethylene glycol while allowing the agglomerated particles to obtain a certain cohesive strength, high density and fluidity, and at the same time, part of WC and VC react to form V4WC5 phase. The heat treatment temperature is 1185°C, and the insulation time is 90 minutes. Then, the particles with too large and too small particle sizes in the heat-treated powder are removed by airflow classification to obtain the WC-V4WC5-Co spherical composite powder with a particle size distribution of 10-30 μm required for printing. Its morphology is as follows Figure 1 (b) The results of physical phase detection are as follows Figure 2 As shown in (a). The powder after classification in the above steps is used as raw material, and the powder spreading type selective laser melting equipment is used for printing and forming, so that WC and V4WC5 form VWC2 phase in situ under the action of laser. The laser printing process parameters used are: laser power 120W, scanning rate 900mm / s, scanning spacing 0.04mm, and powder layer thickness 0.03mm. The phase detection results of laser printed cemented carbide are shown in Figure 2 (b) As shown. The WC-VC-Co parts obtained by printing were subjected to atmosphere protection heat treatment at a temperature of 1410°C. When the temperature reached the target temperature, 5MPa of argon was introduced and kept at this pressure for 50 minutes to decompose the VWC2 phase into WC and V4WC5, and to promote the oriented growth of the formed WC. After cooling to room temperature, a cemented carbide part with a needle-like structure and freely designable shape was obtained. Figure 2 (c) and Figure 3 (b) shows the phase detection results of cemented carbide after laser printing and heat treatment, and the microstructure of cemented carbide with needle-like structure. The volume content of the needle-like structure is about 51%, and the average length of the needle-like WC phase is 1.89 μm and the diameter is 0.28 μm.

[0024] Example 3

[0025] WC, Co and VC powders with an average particle size of less than 1 μm are used as raw materials. The mass fraction of VC in the obtained WC-VC-Co composite powder is 15%, and the mass fraction of Co is 12%. The powder is fully wet-milled with anhydrous ethanol as the medium to ensure that the three raw material powders are evenly mixed and then dried. The dried powder is mixed with deionized water and polyethylene glycol in proportion to form a slurry, and agglomerated and granulated by a high-speed centrifugal atomization drying process to obtain WC-VC-Co spherical composite powder. The spherical composite powder obtained in the above steps is heat-treated to remove polyethylene glycol while allowing the agglomerated particles to obtain a certain cohesive strength, high density and fluidity, and at the same time, part of WC and VC react to form V4WC5 phase. The heat treatment temperature is 1185°C, and the insulation time is 90 minutes. Then, the particles with too large and too small particle sizes in the heat-treated powder are removed by airflow classification to obtain the WC-V4WC5-Co spherical composite powder with a particle size distribution of 10-30 μm required for printing. Its morphology is as follows Figure 1 (c) Phase detection results are as follows Figure 2 (a) As shown. The powder after classification in the above steps is used as raw material, and the powder spreading type selective laser melting equipment is used for printing and forming, so that WC and V4WC5 form VWC2 phase in situ under the action of laser. The laser printing process parameters used are: laser power 130W, scanning rate 800mm / s, scanning spacing 0.04mm, and powder layer thickness 0.03mm. The phase detection results of laser printed cemented carbide are shown in Figure 2 (b) As shown. The WC-VC-Co parts obtained by printing were subjected to atmosphere protection heat treatment at a temperature of 1410°C. When the temperature reached the target temperature, 5MPa of argon was introduced and kept at this pressure for 50 minutes to decompose the VWC2 phase into WC and V4WC5, and to promote the oriented growth of the formed WC. After cooling to room temperature, a cemented carbide part with a needle-like structure and freely designable shape was obtained. Figure 2 (c) and Figure 3 (c) are the phase detection results of cemented carbide after laser printing and heat treatment, and the microstructure of cemented carbide with needle-like structure obtained, where the volume content of needle-like structure is about 60%, the average length of needle-like WC phase is 2.14μm, and the diameter is 0.3μm.

Claims

1. A method for preparing a cemented carbide having a needle-like structure, It is characterized in that The following steps are involved: (1) Using WC, Co and VC powders with an average particle size of less than 1 μm as raw materials, the WC-VC-Co composite powder is prepared so that the mass fraction of VC is 5%-22% and the mass fraction of Co is 10%-20%, and the powder is fully wet-milled with anhydrous ethanol as a medium to ensure that the three raw material powders are evenly mixed and then dried; the dried powder is mixed with deionized water and polyethylene glycol to form a slurry, and agglomerated and granulated by a high-speed centrifugal atomization drying process to obtain a WC-VC-Co spherical composite powder; (2) The spherical composite powder obtained in the above steps is subjected to heat treatment to remove the polyethylene glycol while allowing the agglomerated particles to obtain a certain cohesive strength, high density and fluidity, and to react part of WC and VC to generate V 4 WC 5 phase; the heat treatment temperature is 1180-1250℃, and the holding time is 90-120min; then, the particles with too large and too small particle sizes in the heat-treated powder are removed by airflow classification to obtain WC-V with a particle size distribution of 10-30μm required for printing. 4 WC 5 -Co spherical composite powder; (3) Using the powder classified in the above steps as raw material, a powder spreading type selective laser melting device is used for printing and forming, so that WC and V 4 WC 5 In situ formation of VWC under laser action 2 Phase; The laser printing process parameters used are: laser power 100-140W, scanning rate 800-1000mm / s, scanning spacing 0.04mm, powder layer thickness 0.03mm; (4) The WC-VC-Co parts obtained by printing are subjected to atmosphere protection heat treatment at a temperature of 1410-1480°C. When the temperature rises to the target temperature, 5-6MPa argon gas is introduced and kept at this pressure for 50-80 minutes to make the VWC 2 Phase decomposition into WC and V 4 WC 5 , and promote the oriented growth of the formed WC. After cooling to room temperature, a cemented carbide part with a needle-like structure and freely designable shape is obtained.

2. The method according to claim 1, It is characterized in that In step (3), the phases of the powder formed into parts under the action of laser include: VWC 2 and relatively small amounts of WC, W 2 C.Co 3 W 3 C.

3. The method according to claim 1, It is characterized in that Step (4) The phases after heat treatment of the parts include: WC, V 4 WC 5 、VWC 2 and Co.

4. The method according to claim 1, It is characterized in that The volume content of the needle-like structure in the final part is 40%-70%, the average length of the needle-like WC grains is 1.0-2.2μm, and the average diameter ranges from 0.1-0.3μm.

5. A cemented carbide with needle-like structure prepared according to the method described in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Method for preparing compact nanocrystalline WC-Co hard alloy block material with small grain size

    CN102071346A

  • Fine pure plate-shaped grain cemented carbide and preparation method thereof

    CN103045887A

  • 3D printing preparation method of high-density hard alloy block

    CN113953517A

  • Laser additive manufacturing method for hard alloy with layered structure

    CN117900508A

  • Powder material, powder material for additive manufacturing, and method for producing powder material